High-nitrogen high-entropy alloy ultra-thin strip and preparation method and application thereof
Through high proportion of nitrogen elements and asynchronous rolling technology, high-nitrogen high-entropy alloy extremely thin strips were prepared, which solved the problem of insufficient performance of metal extremely thin strips in the existing technology, achieved efficient mechanical performance improvement, and was suitable for multiple high-ends Application field.
Patent Information
- Application Number
- CN202411085992.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Existing metal ultra-thin belts are difficult to meet the increasing demand for use, especially in the performance research and application of ultra-thin belts of high-entropy alloys.
Using a high proportion of nitrogen to improve the rolling ductility of alloys, the asynchronous rolling parameters are adjusted through multi-pass asynchronous rolling and annealing treatment, and a thin strip of high-nitrogen high-entropy alloy with a thickness of 40-60μm is prepared, with excellent advantages. comprehensive mechanical properties.
A high-nitrogen high-entropy alloy extremely thin belt with low raw material cost has been obtained, with high yield strength, tensile strength, uniform elongation and total elongation, and is suitable for power electronic equipment, aerospace, marine engineering and other fields.
Smart Images

Figure CN119056876A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultra-thin metal strips, and in particular to an ultra-thin high-nitrogen high-entropy alloy strip and a preparation method and application thereof. Background Art
[0002] At present, ultra-thin metal strips have extensive and important applications in my country's industrial production and people's daily lives. For example, copper-nickel alloys and nickel-chromium alloys have high resistivity and heat resistance, and their foils are often used to manufacture precision resistors and strain gauges; tungsten and molybdenum materials still have high strength and hardness at high temperatures, and their foils can be used to manufacture heating devices and electronic tubes; austenitic stainless steel ultra-thin strips have excellent corrosion resistance, formability and good comprehensive mechanical properties, and their thin strip products are often used in aerospace, electronic communications, instrumentation and other fields.
[0003] Ultra-thin metal strips are usually used as structural and functional integrated materials, and their preparation methods include calendering, strip throwing, continuous casting and rolling, etc. Among them, the calendering method has the advantages of high production efficiency, low cost, and excellent product performance.
[0004] Currently, the commonly used ultra-thin metal strips include ordinary nickel silver strips, iron nickel silver strips, manganese nickel silver strips, zinc nickel silver strips and aluminum nickel silver strips, etc. However, with the rapid development of ultra-thin metal strips, the existing ultra-thin metal strips are difficult to meet the increasingly high usage requirements.
[0005] High entropy alloys are usually composed of multiple main elements in equimolar ratios or nearly equimolar ratios, and have a variety of special effects, such as high entropy effect, lattice distortion effect, hysteresis diffusion effect and cocktail effect. Compared with metal ultra-thin strips, ultra-thin high entropy alloys have excellent mechanical properties, corrosion resistance and excellent thermal stability. These characteristics make ultra-thin high entropy alloys have broad application prospects in electronics, optoelectronics, computers, precision machinery manufacturing, robot manufacturing and other industries. The relevant properties of ultra-thin high entropy alloys need to be studied urgently, which shows that the research field of ultra-thin high entropy alloys is broad and has huge development potential.
[0006] Therefore, it is of great significance to develop an ultra-thin strip of high entropy alloy.
[0007] In view of this, the present invention is proposed. Summary of the invention
[0008] The first purpose of the present invention is to provide a method for preparing an ultra-thin strip of a high-nitrogen high-entropy alloy. Based on the property that a high proportion of nitrogen improves the rolling ductility of the alloy, an asynchronous rolling method is used to regulate the asynchronous rolling parameters to obtain an ultra-thin strip of a high-nitrogen high-entropy alloy with excellent comprehensive mechanical properties and low raw material cost, which is beneficial to the development and application of the ultra-thin strip of a high-entropy alloy.
[0009] A second object of the present invention is to provide an ultra-thin strip of high-nitrogen high-entropy alloy.
[0010] The third object of the present invention is to provide an application of a high-nitrogen high-entropy alloy ultra-thin strip in transportation, power electronic equipment, aerospace, marine engineering, medical equipment, precision machinery manufacturing and robot manufacturing.
[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0012] The present invention first provides a method for preparing an ultra-thin strip of a high-nitrogen high-entropy alloy, comprising the following steps:
[0013] A high nitrogen high entropy alloy with a thickness of 1 to 10 mm is subjected to multiple asynchronous rolling to obtain an ultra-thin high nitrogen high entropy alloy strip with a thickness of 40 to 60 μm;
[0014] Wherein, the number of passes of the multi-pass asynchronous rolling is at least 10;
[0015] The total deformation of the multi-pass asynchronous rolling is 94% to 99.6%;
[0016] The roller speed ratio of the upper roller and the lower roller in the multi-pass asynchronous rolling is 1.5 to 2.0:1;
[0017] The high nitrogen high entropy alloy is prepared from the following elements in molar percentage: Fe 46.3% to 47.3%, Mn 29.5% to 30.5%, Co 9.5% to 10.5%, Cr 9.5% to 10.5% and N 3% to 3.9%.
[0018] Furthermore, during the multi-pass asynchronous rolling process, the deformation amount of each rolling pass in the 1st to 3rd passes is 19% to 21%, the deformation amount of each rolling pass in the 4th to 5th passes is 9% to 11%, the deformation amount of each rolling pass in the 6th to 8th passes is 4% to 6%, and the deformation amount of each rolling pass in the 9th to 10th passes and above is 1.5% to 3%.
[0019] Furthermore, the linear speed of the upper roller in the multi-pass asynchronous rolling is 42-56 mm / s, and the linear speed of the lower roller is 20-35 mm / s.
[0020] Furthermore, the temperature of the multi-pass asynchronous rolling is 15-35°C.
[0021] Furthermore, the method for preparing the ultra-thin high-nitrogen high-entropy alloy strip also includes an annealing step, specifically: annealing the ultra-thin high-nitrogen high-entropy alloy strip that has undergone the multiple asynchronous rolling passes at 740-760° C. for 2-5 min.
[0022] Furthermore, after the high nitrogen high entropy alloy ultra-thin strip is annealed at 740-760° C. for 2-5 min, the uniform elongation is ≥9% and the total elongation is ≥10.5%.
[0023] Furthermore, after the high nitrogen high entropy alloy ultra-thin strip is annealed at 740-760° C. for 2-5 min, the yield strength is ≥930 MPa and the tensile strength is ≥1100 MPa.
[0024] Furthermore, the preparation method of the high nitrogen high entropy alloy includes: smelting raw materials containing Fe, Co, Mn, Cr and N elements to obtain a liquid alloy; casting the liquid alloy to obtain an ingot; and sequentially hot forging, hot rolling, solution treatment and cutting the ingot to obtain the high nitrogen high entropy alloy.
[0025] Furthermore, the hot forging temperature is 1050-1130°C.
[0026] Furthermore, the initial temperature of the hot rolling is 1030-1100°C, and the final rolling temperature is 900-1000°C; the hot rolling method includes multiple hot rolling passes, the number of passes of the multiple hot rolling passes is ≥5 times, the deformation of each hot rolling pass is ≥10%, and the total deformation of the multiple hot rolling passes is ≥50%.
[0027] The present invention further provides a high nitrogen high entropy alloy ultra-thin strip, which is prepared by the preparation method of the high nitrogen high entropy alloy ultra-thin strip;
[0028] Wherein, the thickness of the high nitrogen high entropy alloy ultra-thin strip is 40 to 60 μm;
[0029] The high nitrogen high entropy alloy is composed of the following elements in molar percentage: Fe 46.3% to 47.3%, Co 9.5% to 10.5%, Mn 29.5% to 30.5%, Cr 9.5% to 10.5% and N 3% to 3.9%.
[0030] The present invention also provides applications of the high-nitrogen high-entropy alloy ultra-thin strip in transportation, power electronics equipment, aerospace, marine engineering, medical equipment, precision machinery manufacturing, and robot manufacturing.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The preparation method of the high-nitrogen high-entropy alloy ultra-thin strip provided by the present invention is based on the characteristic that a high proportion of nitrogen improves the rolling ductility of the alloy. By utilizing asynchronous rolling means and regulating the parameters of multiple asynchronous rolling passes, a high-nitrogen high-entropy alloy ultra-thin strip with excellent comprehensive mechanical properties and low raw material cost can be obtained, which is conducive to the high-entropy alloy ultra-thin strip playing an important role in the fields of power electronic equipment, aerospace, marine engineering, etc., and provides strong support for the development of related fields.
[0033] (2) The method for preparing the ultra-thin strip of high-nitrogen high-entropy alloy provided by the present invention can obtain an ultra-thin strip of high-nitrogen high-entropy alloy with a thickness of 40 to 60 μm. After annealing, the ultra-thin strip not only has high yield strength and tensile strength, but also has high uniform elongation and total elongation, showing excellent comprehensive mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 This is a picture of the ultra-thin strip of high nitrogen high entropy alloy prepared in Example 1 provided by the present invention;
[0036] Figure 2 A comparison diagram of engineering stress-strain curves of the ultra-thin high-nitrogen high-entropy alloy strip (referred to as rolled state) obtained in step (2) of Example 1 provided by the present invention and the ultra-thin high-nitrogen high-entropy alloy strip (referred to as annealed state) obtained in step (3);
[0037] Figure 3 XRD comparison diagram of the high nitrogen high entropy alloy ultra-thin strip (referred to as rolled state) obtained in step (2) of Example 1 provided by the present invention and the high nitrogen high entropy alloy ultra-thin strip (referred to as annealed state) obtained in step (3);
[0038] Figure 4 This is a SEM image of the ultra-thin strip of high nitrogen high entropy alloy obtained in step (2) of Example 1 provided by the present invention;
[0039] Figure 5 This is a SEM image of the ultra-thin high-nitrogen high-entropy alloy strip after annealing obtained in step (3) of Example 1 provided by the present invention. DETAILED DESCRIPTION
[0040] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If the specific conditions are not indicated in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0041] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0042] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0043] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0044] In a first aspect, the present invention provides a method for preparing an ultra-thin strip of a high-nitrogen high-entropy alloy, comprising the following steps:
[0045] A high nitrogen high entropy alloy with a thickness of 1 to 10 mm is subjected to multiple asynchronous rolling to obtain an ultra-thin high nitrogen high entropy alloy strip with a thickness of 40 to 60 μm.
[0046] Among them, the thickness of the high nitrogen high entropy alloy includes but is not limited to any point value of 1mm, 2mm, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, and 10mm, or a range value between any two of them.
[0047] The thickness of the ultra-thin strip of high nitrogen high entropy alloy includes but is not limited to any point value of 40μm, 43μm, 45μm, 48μm, 50μm, 52μm, 55μm, 58μm, 60μm or a range value between any two of them.
[0048] Among them, the high nitrogen high entropy alloy is subjected to solid solution treatment to homogenize the alloy.
[0049] Wherein, the number of passes of the multi-pass asynchronous rolling is at least 10 times, for example, 10 times, 11 times, 12 times, 13 times, 14 times, 15 times or more.
[0050] The total deformation of the multiple asynchronous rolling is 94% to 99.6%, including but not limited to any point value of 94%, 94.3%, 94.5%, 94.8%, 95%, 95.3%, 95.5%, 95.8%, 96%, 96.5%, 97%, 97.5%, 98%, 98.5%, 99%, 99.3%, 99.5%, 99.6% or the range value between any two of them.
[0051] The roller speed ratio of the upper roller and the lower roller in the multi-pass asynchronous rolling is 1.5 to 2.0:1, including but not limited to any point value of 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1 or a range value between any two of them.
[0052] The high nitrogen high entropy alloy is made of the following elements in molar percentage: Fe 46.3% to 47.3%, Mn 29.5% to 30.5%, Co 9.5% to 10.5%, Cr 9.5% to 10.5% and N 3% to 3.9%. The applicant found that when the nitrogen content in the high nitrogen high entropy alloy is 3% to 3.9%, the ductility of the high nitrogen high entropy alloy is greatly improved.
[0053] Wherein, Fe includes but is not limited to any one of 46.3%, 46.5%, 46.8%, 47%, 47.1%, 47.3% or any range between two of them in terms of mole percentage; Mn includes but is not limited to any one of 29.5%, 29.8%, 30%, 30.2%, 30.5% or any range between two of them in terms of mole percentage; Co includes but is not limited to 9.5%, 9.7%, 9.8%, 10%, 10.2%, 11.8%, 12.6%, 13.9%, 14.1%, 15.3%, 16.4%, 17.6%, 18.7%, 19.8%, 20.9%, 21.4%, 22.9%, 23.4%, 24.5%, 25.6%, 26.7%, 27.8%, 28.9%, 29.9%, 20.1%, 21.2%, 22.3%, 23.4%, 24.6%, 25.7%, 26.8%, 27.9%, 28.8%, 29.9%, 20.1%, 21.4%, 29. The point value of any one of 10.3%, 10.5% or the range between any two of them; the point value of Cr in mole percentage includes but is not limited to 9.5%, 9.8%, 10%, 10.3%, 10.5% or the range between any two of them; the point value of N in mole percentage includes but is not limited to 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9% or the range between any two of them.
[0054] The preparation method of the high-nitrogen high-entropy alloy ultra-thin strip provided by the present invention is based on the property that high proportion of nitrogen improves the rolling ductility of the alloy, and uses asynchronous rolling means to adjust the parameters of multiple asynchronous rolling passes to obtain a high-nitrogen high-entropy alloy ultra-thin strip with excellent comprehensive mechanical properties and low raw material cost, which is conducive to the high-entropy alloy ultra-thin strip playing an important role in power electronic equipment, aerospace, marine engineering and other fields. The application of high-entropy alloy ultra-thin strips will be more extensive, providing strong support for the development of related fields.
[0055] Specifically, the present invention performs multiple asynchronous rolling on a high nitrogen high entropy alloy of a specific composition. Due to the addition of a specific amount of interstitial atoms N in the high nitrogen high entropy alloy, while improving the yield strength, tensile strength and Vickers hardness, the rolling ductility of the alloy is greatly improved, and its rolling deformation can reach 99.8%. Based on this, the present invention performs asynchronous rolling on a high nitrogen high entropy alloy with a thickness of 1 to 10 mm with a reduction of 94% to 99.6% through multiple asynchronous rolling, and obtains an ultra-thin strip of a high nitrogen high entropy alloy with a thickness of 40 to 60 μm. After annealing, the ultra-thin strip not only has high yield strength and tensile strength, but also has high uniform elongation and total elongation, showing excellent comprehensive mechanical properties.
[0056] In some specific embodiments, in order to further improve the comprehensive mechanical properties of the ultra-thin strip of high nitrogen high entropy alloy, in the process of the multi-pass asynchronous rolling, the deformation amount of each rolling in the 1st to 3rd passes (i.e., the 1st, 2nd and 3rd passes) is 19% to 21%, including but not limited to any point value of 19%, 19.5%, 20%, 20.5%, 21% or any range value between the two; the deformation amount of each rolling in the 4th and 5th passes is 9% to 11%, including but not limited to any point value of 9%, 9.5%, 10%, 10.5%, 11%. The rolling deformation of each pass in the 6th to 8th passes (i.e., the 6th, 7th and 8th passes) is 4% to 6%, including but not limited to any one of 4%, 4.5%, 5%, 5.5%, 6% or any range between them; the rolling deformation of each pass in the 9th and 10th and above passes is 1.5% to 3%, including but not limited to any one of 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.3%, 2.5%, 2.8%, 3% or any range between them. Among them, and above passes refer to more than 10 passes, such as the 11th, 12th, 13th, 15th, etc.
[0057] In some specific embodiments, in order to further improve the comprehensive mechanical properties of the ultra-thin strip of high nitrogen high entropy alloy, the linear speed of the upper roller of the multi-pass asynchronous rolling is 42 to 56 mm / s, including but not limited to 42 mm / s, 43 mm / s, 44 mm / s, 45 mm / s, 46 mm / s, 47 mm / s, 48 mm / s, 49 mm / s, 50 mm / s, 51 mm / s, 52 mm / s, 53 mm / s, 54 mm / s, 55 mm / s, 56 mm / s, any point value of mm / s or the range value between any two of them; the linear speed of the lower roller of the multi-pass asynchronous rolling is 20-35mm / s, including but not limited to any point value of 20mm / s, 21mm / s, 22mm / s, 23mm / s, 24mm / s, 25mm / s, 26mm / s, 28mm / s, 30mm / s, 31mm / s, 32mm / s, 33mm / s, 35mm / s or the range value between any two of them.
[0058] In some specific embodiments, the temperature of the multiple asynchronous rolling is 15-35°C, including but not limited to any point value of 15°C, 18°C, 20°C, 22°C, 23°C, 25°C, 27°C, 28°C, 30°C, 33°C, 35°C or a range value between any two of them.
[0059] In some specific embodiments, the multi-pass asynchronous rolling is performed at room temperature.
[0060] In some specific embodiments, in order to further improve the comprehensive mechanical properties of the ultra-thin high nitrogen high entropy alloy strip, the preparation method of the ultra-thin high nitrogen high entropy alloy strip further includes an annealing step, specifically: annealing the ultra-thin high nitrogen high entropy alloy strip with a thickness of 40 to 60 μm at 740 to 760°C for 2 to 5 minutes, and then quenching. The quenching method includes water cooling, and the water cooling is to room temperature, for example, 20 to 30°C.
[0061] In some specific embodiments, after the ultra-thin strip of high nitrogen high entropy alloy is annealed at 740-760°C for 2-5 minutes, the uniform elongation of the obtained ultra-thin strip is ≥9%, and the total elongation is ≥10.5%. Wherein, the uniform elongation includes but is not limited to any point value of 9%, 9.2%, 9.5%, 9.8%, 10%, 10.3%, 10.5%, 10.8%, 11%, 11.2%, 11.5%, 11.7%, 12% or any range value between two of them; the total elongation includes but is not limited to any point value of 10.5%, 10.8%, 11%, 11.2%, 11.4%, 11.5%, 11.7%, 11.9%, 12%, 12.5% or any range value between two of them.
[0062] Among them, uniform elongation refers to the engineering strain value when the strength reaches the maximum (tensile strength) in the tensile curve as the loading progresses. Total elongation, also known as maximum elongation, refers to the strain value corresponding to the end of the tensile curve when the material breaks.
[0063] In some specific embodiments, after the ultra-thin strip of high nitrogen high entropy alloy is annealed at 740-760°C for 2-5 min, the yield strength of the obtained ultra-thin strip is ≥930MPa, including but not limited to any point value of 930MPa, 935MPa, 940MPa, 945MPa, 950MPa, 960MPa, 965MPa, 970MPa, 980MPa, 990MPa, and 1000MPa, or a range value between any two of them.
[0064] In some specific embodiments, after the ultra-thin strip of high nitrogen high entropy alloy is annealed at 740-760°C for 2-5 min, the tensile strength of the obtained ultra-thin strip is ≥1100 MPa, including but not limited to any point value of 1100 MPa, 1105 MPa, 1110 MPa, 1120 MPa, 1130 MPa, 1140 MPa, 1150 MPa, 1160 MPa, 1170 MPa, 1180 MPa, 1190 MPa, 1195 MPa, and 1200 MPa, or a range value between any two of them.
[0065] In some specific embodiments, the preparation method of the high nitrogen high entropy alloy includes: smelting raw materials containing Fe, Co, Mn, Cr and N elements to obtain a liquid alloy; casting the liquid alloy to obtain an ingot; and sequentially hot forging, hot rolling, solution treatment and cutting the ingot to obtain the high nitrogen high entropy alloy.
[0066] In some specific embodiments, the hot forging temperature is 1050-1130°C, including but not limited to any one of 1050°C, 1060°C, 1080°C, 1100°C, 1120°C, 1130°C or a range between any two of them.
[0067] In some specific embodiments, the initial temperature of the hot rolling is 1030-1100°C, including but not limited to any one of 1030°C, 1040°C, 1050°C, 1060°C, 1080°C, and 1100°C or a range between any two of them; the final rolling temperature of the hot rolling is 900-1000°C, including but not limited to any one of 900°C, 910°C, 920°C, 930°C, 950°C, 960°C, and 980°C or a range between any two of them.
[0068] In some specific embodiments, the hot rolling method includes multiple hot rolling, the number of passes of the multiple hot rolling is ≥5, including but not limited to any point value of 5, 6, 7, 8 or any range value between two of them; the deformation of each hot rolling is ≥10%, including but not limited to any point value of 10%, 11%, 12%, 13%, 14%, 15% or any range value between two of them; the total deformation of the multiple hot rolling is ≥50%, including but not limited to any point value of 50%, 51%, 52%, 53%, 54%, 55% or any range value between two of them. Preferably, the deformation of each hot rolling is >10%, and the total deformation of the multiple hot rolling is >50%.
[0069] In some specific embodiments, the raw materials containing Fe, Co, Mn, Cr and N elements include: pure iron blocks, pure cobalt blocks, pure manganese blocks, pure chromium blocks, chromium nitride and manganese nitride alloys, wherein the nitrogen content in the chromium nitride alloy is 10wt.%, the nitrogen content in the manganese nitride alloy is 14.5wt.%, and the purity of the pure iron block, pure cobalt block, pure manganese block, pure chromium block and manganese nitride alloy is each independently 99.9wt.%.
[0070] In some specific embodiments, the smelting refers to vacuum induction smelting in a pressurized vacuum medium frequency induction furnace. Preferably, the vacuum degree of the smelting is 3-5 Pa, the smelting temperature is 1650-1750° C., the smelting time is 15-30 min, and the number of smelting is 4-6 times.
[0071] In some specific implementations, the casting temperature is 1650-1750° C., the casting time is 80-100 seconds, a cylindrical ingot is obtained after the casting, and the mold used for the casting is high-temperature alloy steel.
[0072] In some specific implementations, the hot forging time is 10 to 20 minutes, and a primary alloy billet with a rectangular cross section (105 mm×50 mm) is obtained after the hot forging, and the hot forging is performed in a box furnace.
[0073] In some specific embodiments, the hot rolling device is Two-roll (asynchronous) hot rolling experimental mill, in which the mill roll diameter is 0.45m.
[0074] In some specific implementations, the temperature of the solution treatment is 1150-1250° C., and the time is 2-4 hours.
[0075] In some specific embodiments, after the solution treatment is completed, the product after the solution treatment is cooled to obtain a secondary alloy billet, wherein the cooling method is water cooling; the water cooling temperature is room temperature, such as 20-30°C.
[0076] In some specific implementations, the cutting method includes: using an electric spark wire cutting machine to process the solid solution alloy after the solid solution treatment to a thickness of 1 to 10 mm.
[0077] In some specific implementations, the multi-pass asynchronous rolling is performed by exchanging the head and tail of the rolled plates in each pass and feeding them into the rolling mill for engagement.
[0078] In some specific implementations, the multi-pass asynchronous rolling may adopt any asynchronous rolling mill commonly used in the art, such as a four-roller asynchronous rolling mill, but is not limited thereto.
[0079] In a second aspect, the present invention provides an ultra-thin strip of high-nitrogen high-entropy alloy, which is prepared by the above-mentioned method for preparing the ultra-thin strip of high-nitrogen high-entropy alloy.
[0080] Among them, the thickness of the high-nitrogen high-entropy alloy ultra-thin strip is 40 to 60 μm, including but not limited to any point value of 40 μm, 43 μm, 45 μm, 48 μm, 50 μm, 52 μm, 55 μm, 58 μm, and 60 μm, or a range value between any two of them.
[0081] The high-nitrogen high-entropy alloy ultra-thin strip prepared by the present invention has a small thickness and can be used in the fields of electronics, optoelectronics, computers, precision machinery manufacturing, robot manufacturing, etc., and has broad application prospects.
[0082] The high nitrogen high entropy alloy is composed of the following elements in molar percentage: Fe 46.3% to 47.3%, Co 9.5% to 10.5%, Mn 29.5% to 30.5%, Cr 9.5% to 10.5% and N 3% to 3.9%. Among them, Fe in molar percentage includes but is not limited to any point value of 46.3%, 46.5%, 46.8%, 47%, 47.1%, 47.3% or any range value between two of them; Mn in molar percentage includes but is not limited to any point value of 29.5%, 29.8%, 30%, 30.2%, 30.5% or any range value between two of them; Co in molar percentage includes but is not limited to 9.5%, 9.7%, 9.8%, 10%, 10.2%, The point value of any one of 10.3%, 10.5% or the range between any two of them; the point value of Cr in mole percentage includes but is not limited to 9.5%, 9.8%, 10%, 10.3%, 10.5% or the range between any two of them; the point value of N in mole percentage includes but is not limited to 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9% or the range between any two of them.
[0083] In a third aspect, the present invention also provides applications of the above-mentioned ultra-thin high-nitrogen high-entropy alloy strip in transportation, power electronics equipment, aerospace, marine engineering, medical equipment, precision machinery manufacturing, and robot manufacturing.
[0084] High entropy alloy ultra-thin strips combine the advantages of metal ultra-thin strips and high entropy alloys. High entropy alloys have a variety of special effects, such as high entropy effect, lattice distortion effect, hysteresis diffusion effect and cocktail effect. These characteristics make high entropy alloy ultra-thin strips have broad application prospects in electronics, optoelectronics, computers, precision machinery manufacturing, robotics manufacturing and other industries.
[0085] The high-entropy alloy ultra-thin strip provided by the present invention has excellent comprehensive mechanical properties and low cost, which is conducive to the high-entropy alloy ultra-thin strip playing an important role in power electronic equipment, aerospace, marine engineering and other fields.
[0086] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0087] Example 1
[0088] The Fe 46.8Mn 30 Co 10 Cr 10 N 3.2 A method for preparing an ultra-thin strip of a high-nitrogen high-entropy alloy comprises the following steps:
[0089] (1) Smelting raw materials containing Fe, Co, Mn, Cr and N elements to obtain a liquid alloy. The raw materials containing Fe, Co, Mn, Cr and N elements are: pure iron block, pure cobalt block, pure manganese block, pure chromium block, chromium nitride and manganese nitride alloy, wherein the nitrogen content in the chromium nitride alloy is 10wt.%, the nitrogen content in the manganese nitride alloy is 14.5wt.%, and the purity of the pure iron block, pure cobalt block, pure manganese block, pure chromium block and manganese nitride alloy is independently 99.9wt.%; the amount of raw materials used satisfies the molar percentages of the elements Fe, Co, Mn, Cr and N contained in the following manner: Fe 46.8%, Mn 30.0%, Co 10.0%, Cr 10.0% and N 3.2%. The smelting is carried out by vacuum induction melting in a pressurized vacuum medium frequency induction furnace; the vacuum degree of the smelting is 4 Pa, the smelting temperature is 1700° C., the smelting time is 18 min, and the number of smelting times is 5 times.
[0090] The above liquid alloy is sequentially cast, hot forged, hot rolled, solution treated and cut to obtain a high nitrogen high entropy alloy with a thickness of 1 mm. The casting temperature is 1700°C, the casting time is 90s, and a cylindrical ingot is obtained after casting. The mold used for casting is high temperature alloy steel. The hot forging temperature is 1100°C, the hot forging time is 10min, and a primary alloy billet with a rectangular cross-section (105mm×50mm) is obtained after hot forging. The hot forging is carried out in a box furnace. The initial temperature of hot rolling is 1050°C, the final rolling temperature is 950°C, the hot rolling method is multi-pass hot rolling, the number of hot rolling passes is 5 times, the deformation of each hot rolling pass is 10%, and the total deformation after hot rolling is 50%. After hot rolling, a primary densified alloy billet with a plate thickness of 20 mm is obtained. The hot rolling device is Two-roll (asynchronous) hot rolling experimental mill, where the mill roll diameter is 0.45m. The temperature of the solution treatment is 1200℃, and the time of the solution treatment is 2h; after the solution treatment is completed, the product after the solution treatment is cooled to obtain a secondary alloy billet, where the cooling method is water cooling; the water cooling temperature is room temperature 25℃. The solid solution alloy obtained after the solution treatment is processed to a thickness of 1mm using an electric spark wire cutting machine.
[0091] (2) The high nitrogen high entropy alloy with a thickness of 1 mm obtained in step (1) is subjected to multiple asynchronous rolling to obtain a high nitrogen high entropy alloy ultra-thin strip with a thickness of 50 μm. Among them, the temperature of multi-pass asynchronous rolling is room temperature 25°C, the number of multi-pass asynchronous rolling passes is 10 times, the deformation amount of each rolling pass in the 1st to 3rd passes is 20%, the deformation amount of each rolling pass in the 4th to 5th passes is 10%, the deformation amount of each rolling pass in the 6th to 8th passes is 4%, and the deformation amount of each rolling pass in the 9th to 10th passes is 1.5%. The final total deformation of multi-pass asynchronous rolling is controlled to be 95%. The multi-pass asynchronous rolling process adopts the method of exchanging the head and tail of the rolled plate into the rolling mill for engagement in each pass. The linear speed of the upper roller of the multi-pass asynchronous rolling is 49mm / s, the linear speed of the lower roller is 28mm / s, the roller speed ratio of the upper roller to the lower roller is 1.75:1, and the multi-pass asynchronous rolling device is a four-roller asynchronous rolling mill of Northeastern University.
[0092] After testing, the yield strength, tensile strength, uniform elongation and total elongation of the ultra-thin strip of high nitrogen high entropy alloy obtained in step (2) are 1905 MPa, 1921 MPa, 0.2% and 1.5% respectively.
[0093] (3) The ultra-thin strip of high nitrogen high entropy alloy obtained in step (2) is subjected to a short annealing treatment at a temperature of 750° C. and an annealing holding time of 3 min; and then quenched by water cooling to a temperature of room temperature 25° C.
[0094] After testing, the yield strength, tensile strength, uniform elongation and total elongation of the annealed high-nitrogen high-entropy alloy ultra-thin strip obtained in step (3) are 950 MPa, 1119 MPa, 11.3% and 11.5%, respectively, showing excellent comprehensive mechanical properties.
[0095] like Figure 1 Shown is a physical picture of the high nitrogen high entropy alloy ultra-thin strip obtained in step (2) of this embodiment.
[0096] like Figure 2 The figure shows the engineering stress-strain curve comparison of the ultra-thin strip of high nitrogen high entropy alloy obtained in step (2) of this embodiment (referred to as rolled state) and the ultra-thin strip of high nitrogen high entropy alloy after annealing obtained in step (3) (referred to as annealed state), from which the comparison of the tensile mechanical properties of the two can be seen.
[0097] like Figure 3 Shown is the XRD comparison diagram of the high nitrogen high entropy alloy ultra-thin strip (referred to as rolled state) obtained in step (2) of this embodiment and the high nitrogen high entropy alloy ultra-thin strip (referred to as annealed state) obtained in step (3). It can be seen that both are composed of a single-phase austenite structure and some precipitated phases.
[0098] like Figure 4 The SEM image of the high nitrogen high entropy alloy ultra-thin strip (referred to as rolled state) obtained in step (2) of this embodiment is shown. Figure 5 The figure shows the SEM image of the ultra-thin strip of high nitrogen high entropy alloy (hereinafter referred to as annealed state) after annealing obtained in step (3) of this embodiment. It can be seen that the rolled plate has a strip-like deformation structure, while the annealed plate shows a fine equiaxed crystal structure.
[0099] Example 2
[0100] The Fe 46.8 Mn 30 Co 10 Cr 10 N 3.2 The method for preparing an ultra-thin strip of a high-nitrogen high-entropy alloy comprises the following steps:
[0101] (1) is basically the same as step (1) of Example 1, except that the solid solution alloy obtained after the solid solution treatment is processed to a thickness of 5 mm using an electric spark wire cutting machine.
[0102] (2) The high nitrogen high entropy alloy with a thickness of 5 mm obtained in step (1) is subjected to multiple asynchronous rolling to obtain a high nitrogen high entropy alloy ultra-thin strip with a thickness of 55 μm. Among them, the temperature of multi-pass asynchronous rolling is room temperature 25°C, the number of multi-pass asynchronous rolling passes is 10 times, the deformation of each rolling pass in the 1st to 3rd passes is 21%, the deformation of each rolling pass in the 4th to 5th passes is 10%, the deformation of each rolling pass in the 6th to 8th passes is 4%, and the deformation of each rolling pass in the 9th to 10th passes is 2%. The total deformation of the multi-pass asynchronous rolling is finally controlled to be 99%. The multi-pass asynchronous rolling process adopts the method of exchanging the head and tail of the rolled plate into the rolling mill for engagement in each pass. The linear speed of the upper roller of the multi-pass asynchronous rolling is 48mm / s, the linear speed of the lower roller is 32mm / s, the roller speed ratio of the upper roller to the lower roller is 1.5:1, and the multi-pass asynchronous rolling device is a four-roller asynchronous rolling mill of Northeastern University.
[0103] (3) The ultra-thin strip of high nitrogen high entropy alloy obtained in step (2) is subjected to a short annealing treatment at a temperature of 740° C. and an annealing holding time of 4 min; and then quenched by water cooling to a temperature of room temperature 25° C.
[0104] Example 3
[0105] The Fe 46.8 Mn 30 Co 10 Cr 10 N 3.2 The method for preparing the ultra-thin strip of high nitrogen high entropy alloy comprises the following steps:
[0106] (1) is basically the same as step (1) of Example 1, except that the solid solution alloy obtained after the solid solution treatment is processed to a thickness of 10 mm using an electric spark wire cutting machine.
[0107] (2) The high nitrogen high entropy alloy with a thickness of 10 mm obtained in step (1) is subjected to multiple asynchronous rolling to obtain an ultra-thin high nitrogen high entropy alloy strip with a thickness of 45 μm. Among them, the temperature of multi-pass asynchronous rolling is room temperature 25°C, the number of multi-pass asynchronous rolling passes is 11 times, the deformation of each rolling pass in the 1st to 3rd passes is 19%, the deformation of each rolling pass in the 4th to 5th passes is 9%, the deformation of each rolling pass in the 6th to 8th passes is 6%, and the deformation of each rolling pass in the 9th to 11th passes is 2%. The total deformation of the multi-pass asynchronous rolling is finally controlled to be 99%. The multi-pass asynchronous rolling process adopts the method of exchanging the head and tail of the rolled plate into the rolling mill for engagement in each pass. The linear speed of the upper roller of the multi-pass asynchronous rolling is 54mm / s, the linear speed of the lower roller is 30mm / s, the roller speed ratio of the upper roller to the lower roller is 1.8:1, and the multi-pass asynchronous rolling device is a four-roller asynchronous rolling mill of Northeastern University.
[0108] (3) The ultra-thin strip of high nitrogen high entropy alloy obtained in step (2) is subjected to a short annealing treatment at a temperature of 760° C. and an annealing holding time of 2 min; and then quenched by water cooling to a temperature of room temperature 25° C.
[0109] Example 4
[0110] The Fe 46.8 Mn 30 Co 10 Cr 10 N 3.2 The preparation method of the high nitrogen high entropy alloy ultra-thin strip is basically the same as that in Example 1, except that: in step (2), the deformation amount of each rolling pass in the 1st to 3rd passes is 20%, the deformation amount of each rolling pass in the 4th to 5th passes is 10%, the deformation amount of each rolling pass in the 6th to 8th passes is 4%, and the deformation amount of each rolling pass in the 9th to 10th passes is 2%, and the total deformation amount of the multi-pass asynchronous rolling is finally controlled to be 96%.
[0111] The thickness of the high nitrogen high entropy alloy ultra-thin strip prepared in this embodiment is 40 μm.
[0112] Example 5
[0113] The Fe 46.8 Mn 30 Co 10 Cr 10 N3.2 The preparation method of the high nitrogen high entropy alloy ultra-thin strip is basically the same as that in Example 1, except that: in step (2), the linear speed of the upper roller in the multi-pass asynchronous rolling is 45 mm / s, the linear speed of the lower roller is 28 mm / s, and the roller speed ratio of the upper roller to the lower roller is 1.6:1.
[0114] The thickness of the high nitrogen high entropy alloy ultra-thin strip prepared in this embodiment is 60 μm.
[0115] Example 6
[0116] The Fe 46.8 Mn 30 Co 10 Cr 10 N 3.2 The preparation method of the high nitrogen high entropy alloy ultra-thin strip is basically the same as that in Example 1, except that: in step (2), the linear speed of the upper roller in the multi-pass asynchronous rolling is 53 mm / s, the linear speed of the lower roller is 28 mm / s, and the roller speed ratio of the upper roller to the lower roller is 1.9:1.
[0117] The thickness of the high nitrogen high entropy alloy ultra-thin strip prepared in this embodiment is 40 μm.
[0118] Example 7
[0119] The Fe 465 Mn 295 Co 105 Cr 10 N 35 The method for preparing the ultra-thin strip of high nitrogen high entropy alloy comprises the following steps:
[0120] (1) Smelting raw materials containing Fe, Co, Mn, Cr and N elements to obtain a liquid alloy. The raw materials containing Fe, Co, Mn, Cr and N elements are: pure iron block, pure cobalt block, pure manganese block, pure chromium block, chromium nitride and manganese nitride alloy, wherein the nitrogen content in the chromium nitride alloy is 10wt.%, the nitrogen content in the manganese nitride alloy is 14.5wt.%, and the purity of the pure iron block, pure cobalt block, pure manganese block, pure chromium block and manganese nitride alloy is independently 99.9wt.%; the amount of raw materials used satisfies the molar percentages of the elements Fe, Co, Mn, Cr and N contained in the following manner: Fe 46.5%, Mn 29.5%, Co 10.5%, Cr 10.0% and N 3.5%. The smelting is carried out by vacuum induction melting in a pressurized vacuum medium frequency induction furnace; the vacuum degree of the smelting is 5 Pa, the smelting temperature is 1750° C., the smelting time is 20 min, and the number of smelting times is 5 times.
[0121] The above liquid alloy is sequentially cast, hot forged, hot rolled, solutionized and cut to obtain a high nitrogen high entropy alloy with a thickness of 1 mm. The casting temperature is 1730°C, the casting time is 90s, and a cylindrical ingot is obtained after casting. The mold used for casting is high temperature alloy steel. The hot forging temperature is 1130°C, the hot forging time is 10min, and a primary alloy billet with a rectangular cross-section (105mm×50mm) is obtained after hot forging. The hot forging is carried out in a box furnace. The initial temperature of hot rolling is 1100°C, the final rolling temperature is 900°C, the hot rolling method is multi-pass hot rolling, the number of hot rolling passes is 5 times, the deformation of each hot rolling pass is 11%, and the total deformation after hot rolling is 55%. After hot rolling, a primary densified alloy billet with a plate thickness of 40mm is obtained. The hot rolling device is Two-roll (asynchronous) hot rolling experimental mill, where the mill roll diameter is 0.45m. The temperature of the solution treatment is 1230℃, and the time of the solution treatment is 3h; after the solution treatment is completed, the product after the solution treatment is cooled to obtain a secondary alloy billet, where the cooling method is water cooling; the water cooling temperature is room temperature 25℃. The solid solution alloy obtained after the solution treatment is processed to a thickness of 2mm using an electric spark wire cutting machine.
[0122] (2) The high nitrogen high entropy alloy with a thickness of 2 mm obtained in step (1) is subjected to multiple asynchronous rolling to obtain a high nitrogen high entropy alloy ultra-thin strip with a thickness of 45 μm. Among them, the temperature of multi-pass asynchronous rolling is room temperature 25°C, the number of multi-pass asynchronous rolling passes is 10 times, the deformation of each rolling pass in the 1st to 3rd passes is 20%, the deformation of each rolling pass in the 4th to 5th passes is 10%, the deformation of each rolling pass in the 6th to 8th passes is 4%, and the deformation of each rolling pass in the 9th to 10th passes is 3%. The final total deformation of multi-pass asynchronous rolling is controlled to be 98%. The multi-pass asynchronous rolling process adopts the method of exchanging the head and tail of the rolled plate into the rolling mill for engagement in each pass. The linear speed of the upper roller of the multi-pass asynchronous rolling is 56mm / s, the linear speed of the lower roller is 28mm / s, the roller speed ratio of the upper roller to the lower roller is 2:1, and the multi-pass asynchronous rolling device is a four-roller asynchronous rolling mill of Northeastern University.
[0123] (3) The ultra-thin strip of high nitrogen high entropy alloy obtained in step (2) is subjected to a short annealing treatment at a temperature of 740° C. and an annealing holding time of 4 min; and then quenched by water cooling to a temperature of room temperature 25° C.
[0124] Example 8
[0125] The Fe 46.5 Mn 29.5 Co 10.5 Cr 9.7 N 3.8The preparation method of the high nitrogen high entropy alloy ultra-thin strip is basically the same as that in Example 7, except that: in step (1), the amount of raw materials used satisfies the molar percentages of the elements Fe, Co, Mn, Cr and N contained: Fe 46.5%, Mn 29.5%, Co10.5%, Cr 9.7% and N 3.8%.
[0126] Comparative Example 1
[0127] The Fe 46.8 Mn 30 Co 10 Cr 10 N 3.2 The preparation method of the high nitrogen high entropy alloy ultra-thin strip is basically the same as that in Example 1, except that: in step (2), the number of passes of the multi-pass asynchronous rolling is 9 times, the deformation amount of each rolling pass in the 1st to 2nd passes is 20%, the deformation amount of each rolling pass in the 3rd to 4th passes is 10%, the deformation amount of each rolling pass in the 5th to 7th passes is 4%, and the deformation amount of each rolling pass in the 8th to 9th passes is 2%, and the total deformation amount of the multi-pass asynchronous rolling is finally controlled to be 76%.
[0128] The thickness of the high nitrogen high entropy alloy ultra-thin strip prepared in this comparative example is 240 μm.
[0129] Comparative Example 2
[0130] The Fe 46.8 Mn 30 Co 10 Cr 10 N 3.2 The preparation method of the high nitrogen high entropy alloy ultra-thin strip is basically the same as that in Example 1, except that: in step (2), the linear speed of the upper roller in the multi-pass asynchronous rolling is 84 mm / s, the linear speed of the lower roller is 28 mm / s, and the roller speed ratio of the upper roller to the lower roller is 3.0:1.
[0131] Comparative Example 3
[0132] The Fe 48 Mn 30 Co 10 Cr 10 The preparation method of the N2 alloy ultra-thin strip is basically the same as that of Example 1, except that: in step (1), the amount of raw materials used satisfies the molar percentages of the elements Fe, Co, Mn, Cr and N contained: Fe 48%, Mn 30%, Co 10%, Cr 10% and N2%.
[0133] The thickness of the high nitrogen high entropy alloy ultra-thin strip prepared in this comparative example is 200 μm.
[0134] Comparative Example 4
[0135] The Fe 46.8 Mn 30 Co 10 Cr 10 N 3.2 The preparation method of the ultra-thin alloy strip is basically the same as that in Example 1, except that: no cutting is performed in step (1), that is, in step (2), a high-nitrogen high-entropy alloy with a thickness of 20 mm is directly used for multiple asynchronous rolling.
[0136] The thickness of the high nitrogen high entropy alloy ultra-thin strip prepared in this comparative example is 80 μm.
[0137] Experimental example
[0138] With reference to standard GB / T 228.1-2010, the uniform elongation, total elongation, yield strength and tensile strength of the ultra-thin high nitrogen high entropy alloy strips prepared in each embodiment and each comparative example after annealing were measured, and the results are shown in Table 1.
[0139] Among them, the calculation method of uniform elongation and total elongation is as follows: on the force-extension curve obtained by the extensometer, the elastic extension part is deducted from the total extension at the maximum force, that is, the plastic extension at the maximum force is obtained, and it is divided by the extensometer gauge length to obtain the uniform elongation; on the force-extension curve obtained by the extensometer, the elastic extension part is deducted from the total extension at break, that is, the plastic extension at break is obtained, and it is divided by the extensometer gauge length to obtain the total elongation.
[0140] The yield strength is calculated as follows: On the force-extension curve, draw a line parallel to the elastic straight line segment of the curve, and the distance from this straight line segment on the extension axis is equivalent to the specified plastic elongation, that is, 0.2%. The intersection point of this parallel line and the curve gives the force corresponding to the required yield strength, and this force is divided by the original cross-sectional area of the specimen to obtain the yield strength.
[0141] The calculation method of tensile strength is as follows: On the force-extension curve, draw a parallel line parallel to the force axis and at a distance from the axis equivalent to the uniform elongation. The intersection of this parallel line and the curve gives the force corresponding to the tensile strength. This force is divided by the original cross-sectional area of the specimen to obtain the tensile strength.
[0142] Table 1 Elongation and mechanical properties of each ultra-thin strip
[0143] Group Uniform elongation Total elongation Yield strength / MPa Tensile strength / MPa Example 1 11.3% 11.5% 950 1119 Example 2 9.4% 10.8% 985 1180 Example 3 9.2% 10.5% 996 1195 Example 4 11.0% 11.4% 977 1156 Example 5 11.5% 11.9% 930 1107 Example 6 10.8% 11.2% 965 1130 Example 7 10.9% 11.3% 978 1185 Example 8 10.6% 11.1% 989 1210 Comparative Example 1 19.4% 23.0% 840 927 Comparative Example 2 5.3% 6.7% 963 1125 Comparative Example 3 7.9% 9.1% 782 951 Comparative Example 4 8.5% 9.2% 945 1100
[0144] It can be seen from Table 1 that the high nitrogen high entropy alloy ultra-thin strips prepared in various embodiments of the present invention have excellent comprehensive mechanical properties.
[0145] However, due to insufficient number of asynchronous rolling passes and insufficient total deformation, comparative example 1 cannot be prepared into an ultra-thin metal strip (the thickness is too large).
[0146] In Comparative Example 2, the surface quality of the thin strip material is significantly reduced due to the excessively large roller speed ratio.
[0147] In Comparative Example 3, due to the low nitrogen content, the alloy has insufficient rolling ductility, and thus a thin strip material cannot be obtained (the thickness is too large).
[0148] In Comparative Example 4, since no cutting was performed, a high nitrogen high entropy alloy with a thickness of 20 mm was directly subjected to multiple asynchronous rolling passes, resulting in the alloy material being finally rolled to a thickness of only 80 μm, which is relatively thick.
[0149] In summary, the preparation method of the high-nitrogen high-entropy alloy ultra-thin strip provided by the present invention can obtain a high-nitrogen high-entropy alloy ultra-thin strip with excellent comprehensive mechanical properties, which can meet the use requirements of the high-entropy alloy ultra-thin strip, and can make the application of the high-entropy alloy ultra-thin strip more extensive, providing strong support for the development of related fields.
[0150] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A method for preparing an ultra-thin strip of high nitrogen high entropy alloy, It is characterized in that The steps include: A high nitrogen high entropy alloy with a thickness of 1 to 10 mm is subjected to multiple asynchronous rolling to obtain an ultra-thin high nitrogen high entropy alloy strip with a thickness of 40 to 60 μm; Wherein, the number of passes of the multi-pass asynchronous rolling is at least 10; The total deformation of the multi-pass asynchronous rolling is 94% to 99.6%; The roller speed ratio of the upper roller and the lower roller in the multi-pass asynchronous rolling is 1.5 to 2.0:1; The high nitrogen high entropy alloy is prepared from the following elements in molar percentage: Fe 46.3% to 47.3%, Mn 29.5% to 30.5%, Co 9.5% to 10.5%, Cr 9.5% to 10.5% and N 3% to 3.9%.
2. The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to claim 1, It is characterized in that During the multi-pass asynchronous rolling process, the deformation amount of each rolling pass in the 1st to 3rd passes is 19% to 21%, the deformation amount of each rolling pass in the 4th to 5th passes is 9% to 11%, the deformation amount of each rolling pass in the 6th to 8th passes is 4% to 6%, and the deformation amount of each rolling pass in the 9th to 10th passes and above is 1.5% to 3%.
3. The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to claim 1, It is characterized in that The linear speed of the upper roller in the multi-pass asynchronous rolling is 42-56 mm / s, and the linear speed of the lower roller is 20-35 mm / s.
4. The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to claim 1, It is characterized in that The temperature of the multi-pass asynchronous rolling is 15-35°C.
5. The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to claim 1, It is characterized in that At least one of the following conditions is met: (1) The method for preparing the ultra-thin high nitrogen high entropy alloy strip further comprises an annealing step, specifically: annealing the ultra-thin high nitrogen high entropy alloy strip after the multiple asynchronous rolling at 740-760° C. for 2-5 min; (2) after annealing the ultra-thin strip of high nitrogen high entropy alloy at 740-760° C. for 2-5 min, the uniform elongation is ≥9% and the total elongation is ≥10.5%; (3) After annealing the ultra-thin strip of high nitrogen high entropy alloy at 740-760° C. for 2-5 min, the yield strength is ≥930 MPa and the tensile strength is ≥1100 MPa.
6. The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to claim 1, It is characterized in that The preparation method of the high nitrogen high entropy alloy comprises: smelting raw materials containing Fe, Co, Mn, Cr and N elements to obtain a liquid alloy; casting the liquid alloy to obtain an ingot; and sequentially hot forging, hot rolling, solution treatment and cutting the ingot to obtain the high nitrogen high entropy alloy.
7. The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to claim 6, It is characterized in that The hot forging temperature is 1050-1130°C.
8. The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to claim 6, It is characterized in that The initial temperature of the hot rolling is 1030-1100°C, and the final rolling temperature is 900-1000°C; The hot rolling method comprises multiple hot rolling passes, the number of the multiple hot rolling passes is ≥5 times, the deformation amount of each hot rolling pass is ≥10%, and the total deformation amount of the multiple hot rolling passes is ≥50%.
9. A high nitrogen high entropy alloy ultra-thin strip, It is characterized in that The method for preparing the ultra-thin strip of high nitrogen high entropy alloy according to any one of claims 1 to 8 is used; Wherein, the thickness of the high nitrogen high entropy alloy ultra-thin strip is 40 to 60 μm; The high nitrogen high entropy alloy is composed of the following elements in molar percentage: Fe 46.3% to 47.3%, Co 9.5% to 10.5%, Mn 29.5% to 30.5%, Cr 9.5% to 10.5% and N 3% to 3.9%.
10. Application of the high nitrogen high entropy alloy ultra-thin strip as claimed in claim 9 in transportation, power electronic equipment, aerospace, marine engineering, medical equipment, precision machinery manufacturing and robot manufacturing.
Citation Information
Patent Citations
Preparation method for medium / high-entropy alloy foil of heterogeneous lamellar structure
CN111360074A
Method for preparing high-strength heterogeneous high-entropy alloy through accumulative pack rolling
CN112547798A
High-nitrogen high-entropy alloy and preparation method thereof
CN112575236A
High-toughness low-temperature nickel-free high-entropy alloy and preparation method thereof
CN115572879A
High-entropy alloy and method of its deformation-heat treatment
RU2790708C1