High-temperature continuous drawing method for refractory brittle metal wire
By using conductive electrodes on refractory brittle metal wires for low voltage and high current heating, continuous pulling in red heat state is achieved, solving the problems of complexity and high energy consumption of traditional equipment, improving processing efficiency and plasticity, and suitable for Brittle wire material.
Patent Information
- Application Number
- CN202411201477.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
During the process of continuous thermal pulling of high temperature, traditional equipment is complex and has high energy consumption, resulting in low processing efficiency. The existing technology is mainly suitable for metal wire materials with good plasticity, and cannot effectively treat brittle wire materials.
The conductive electrode is used to contact the refractory brittle metal wire, and the wire drawing is continuously pulled in the red heat state with low voltage and high current, simplifying the equipment and maintaining the high temperature state, and passing through the wire drawing die.
It has achieved simplification of equipment, reduced energy consumption, improved the processing efficiency and plasticity of refractory brittle metal wires, and significantly improved the pass processing rate.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal processing, and in particular relates to a high-temperature continuous drawing method for refractory brittle metal wires. Background Art
[0002] Refractory brittle metals such as iridium-based alloys, tungsten-based alloys, molybdenum-based alloys, and zirconium-based alloys are brittle at room temperature and have high plastic-brittle transition temperatures, so they can only be plastically formed by hot processing. In the manufacturing process of refractory brittle metal wires, traditional processing methods use tubular electric furnaces, tubular gas furnaces, induction coils, etc. as heat sources for high-temperature continuous drawing. The required equipment is relatively complex and has high energy consumption. After the wire is gradually drawn, the cooling speed is accelerated, and a high temperature cannot be maintained before entering the wire drawing die, resulting in a small pass processing rate and low processing efficiency.
[0003] CN201711400640 discloses a production process for continuous drawing and undrawing of copper wire, comprising the following steps: drawing a 3.5 mm copper wire through 13 wire drawing dies to obtain a copper wire A; wherein the diameters of the 13 wire drawing dies are: 2.76-2.78 mm, 2.73-2.75 mm, 2.47-2.49 mm, 2.25-2.27 mm, 2.22-2.24 mm, 2.08-2.10 mm, 2.00-2. 02mm, 1.78-1.80mm, 1.67-1.69mm, 1.38-1.40mm, 1.32-1.34mm, 1.12-1.14mm, 1.12-1.14mm; place copper wire A in an annealing device for annealing to obtain copper wire B; wherein the annealing current is 30-35A, and the annealing speed is 800-1000 rpm; place copper wire B in a heat preservation device for heat preservation, and then wind up and inspect it to obtain it. The present invention increases the specifications of copper wire, slows down the speed of continuous drawing and annealing, and ensures stable product quality and output. The present invention improves the capacity of continuous drawing and annealing of copper wire to ensure that product quality is not affected.
[0004] The above method adopts continuous cold drawing followed by separate continuous annealing, rather than continuous hot drawing at high temperature, and is only suitable for forming metal wires with good plasticity such as copper wire.
[0005] CN202320362595 discloses a copper wire continuous drawing and annealing production line, including a pay-off machine and a take-up machine arranged on both sides, a drawing box, an annealing machine and a tension control box are arranged in sequence between the pay-off machine and the take-up machine, a plurality of winding wheels and a drawing die symmetrically installed on the upper and lower sides of the winding wheels are arranged side by side in the drawing box, the winding wheel includes a small wheel and a large wheel, and winding grooves are processed on the outer rings of the small wheel and the large wheel. The copper wire passes through the drawing die during the reciprocating winding process of the winding grooves of the small wheel and the large wheel, and a contact wheel is arranged in the annealing machine to perform two-stage annealing on the copper wire, and a tension wheel is arranged below the tension control box through shaft rotation. Compared with the prior art, the utility model is a copper wire continuous drawing and annealing production line, in which the copper wire is annealed by the annealing machine during the drawing process, and is naturally cooled at the same time, without the need for back and forth transportation, shortening the processing time and greatly improving the production and processing efficiency.
[0006] The above method uses continuous cold drawing and continuous annealing, not continuous hot drawing of brittle wire at high temperature. The "winding wheel", "contact wheel" and "tension wheel" mentioned in it are only used to change the direction of wire movement or provide tension, and do not play a conductive role. It is also only suitable for forming metal wires with good plasticity such as copper wire.
[0007] CN201910039505 discloses a high-molybdenum medical wire and a processing method thereof in the field of molybdenum wire production technology, and the specific processing method steps are as follows: Step 1: Select metal molybdenum powder as raw material; Step 2: Obtain a shaped square bar or round rod-shaped metal molybdenum rod by a powder metallurgy method and by using an oil press; Step 3: Activate and sinter the molybdenum rod; Step 4: Heat the sintered molybdenum rod to 1400°C and perform rolling, rotary forging and drawing processes; Step 5: Anneal the Mo-La2O3-doped molybdenum wire in a hydrogen protective atmosphere at a temperature of 1000-2000°C; Step 6: Place the annealed molybdenum wire into an electrolytic cell with a continuous multi-stage gap for electrolysis; Step 7: Inspect and package; The production process of the present invention is simple, and the tensile strength, sag resistance, room temperature toughness and plasticity of the produced molybdenum wire are effectively improved, which expands the scope of use of molybdenum wire in medical wires and improves the service life of the molybdenum wire.
[0008] The above method does not mention the specific drawing process. The front-end rolling and rotary forging processes use electromagnetic induction heating, and the heating process and the processing process are still separated. Therefore, the present invention proposes a high-temperature continuous drawing method for refractory brittle metal wires. Summary of the invention
[0009] The object of the present invention is to provide a high-temperature continuous drawing method for refractory brittle metal wires, so that the metal wires are electrically heated and kept in a red-hot state while passing through a wire drawing die, thereby simplifying equipment, reducing energy consumption, and improving processing efficiency.
[0010] To achieve the above object, the present invention provides the following technical solution: a high-temperature continuous drawing method for refractory brittle metal wires, using conductive electrodes to contact the wires passing through both sides of a wire drawing die, passing low voltage and high current, so that the wires pass through the wire drawing die in a red-hot state; the method specifically comprises the following steps:
[0011] S1: Die insertion: Make the head of the refractory brittle metal wire into a wire drawing head, pass it through the wire drawing die coated with high-temperature lubricant, and clamp the wire drawing head with wire clamps;
[0012] S2: Clamping: using conductive electrodes to contact the two ends of the refractory brittle metal wire respectively;
[0013] S3: Power on; low voltage and high current are applied to the metal wire in the middle through the conductive electrode, so that the wire in the middle becomes red hot and reaches the temperature required for hot drawing;
[0014] S4: Continuous drawing: Start the wire drawing equipment and adjust the appropriate speed so that the wire can quickly and continuously reach a red-hot state after entering the contact range of the conductive electrode and before entering the wire drawing die, and the red-hot wire passes through the wire drawing die continuously.
[0015] Preferably, the wire drawing head has a taper, and its diameter is smaller than the metal wire body, can pass through the wire drawing die, can be clamped by the wire clamp, and leaves a sufficient length margin between the wire drawing die and the wire clamp for placing the conductive electrode.
[0016] Preferably, the conductive electrode is a cylindrical conductive block or a conductive roller, which is provided with a tension device so that the wire can be in close contact with it.
[0017] Preferably, the cylindrical conductive block is one of cemented carbide, beryllium bronze, and wear-resistant graphite.
[0018] Preferably, the conductive roller is one of a copper conductive roller, a steel conductive roller, and a graphite conductive roller.
[0019] Preferably, one electrode of the conductive electrode contacts the metal wire that has not entered the wire drawing die, and the other electrode contacts the metal wire between the wire drawing die and the wire clamp, and the distance between the two electrodes is determined according to the drawing speed and the actual required heating time.
[0020] Preferably, the low voltage and high current is low voltage direct current or low voltage alternating current, and the current value is determined according to the wire diameter, the distance between the two electrodes and the plastic-brittle transition temperature of the metal.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention adopts direct electrical heating of the drawn wire, which can simplify the equipment, reduce equipment costs, and reduce energy consumption; the metal wire is kept above the plastic-brittle transition temperature during the process of passing through the drawing die, which can improve the plasticity of the material, increase the pass processing rate, and effectively improve the processing efficiency. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] A high temperature continuous drawing method for refractory brittle metal wire, the specific steps comprising:
[0025] S1: Die insertion: Make a wire drawing head with a length of 10cm and a wire diameter of φ1.80mm~1.85mm with a φ2.00mm iridium alloy wire, pass it through a φ1.90mm wire drawing die coated with high-temperature lubricant, and clamp the wire drawing head with wire clamps;
[0026] S2: Clamping: Wear-resistant graphite electrode blocks are used to contact the two ends of the refractory brittle metal wire. One electrode is located between the wire drawing die and the wire clamp, 5 cm away from the wire drawing die, and the other electrode is located on the other side of the wire drawing die, 95 cm away from the wire drawing die. At this time, the length of the iridium alloy wire between the two electrodes is 100 cm;
[0027] S3: Power on: A 200A direct current is applied to the iridium alloy wire in the middle through the conductive electrode. At this time, the DC voltage is 4.75V. The wire in the middle gradually becomes red hot and reaches 1020℃ after about 15s.
[0028] S4: Continuous drawing: Start the wire drawing equipment and draw at a speed of 5cm / s. After the wire enters the contact range of the conductive electrode, it enters the wire drawing die about 18s later. At this time, the temperature has reached 1020℃ and it passes through the φ1.90mm wire drawing die smoothly at this temperature. The pass processing rate reaches 9.75% and the heating power is 950W.
[0029] Example 2
[0030] A high temperature continuous drawing method for refractory brittle metal wire, the specific steps comprising:
[0031] S1: Die insertion: Make a φ1.00mm molybdenum alloy wire into a drawing head with a length of 10cm and a wire diameter of φ0.80mm~0.85mm, pass it through a φ0.95mm drawing die coated with high-temperature lubricant, and clamp the drawing head with wire clamps;
[0032] S2: Clamping: A copper conductive roller electrode with a tension device is used to contact the two ends of the molybdenum alloy wire respectively. One conductive roller electrode is located between the wire drawing die and the wire clamp, 5 cm away from the wire drawing die, and the other electrode is located on the other side of the wire drawing die, 195 cm away from the wire drawing die. At this time, the length of the molybdenum alloy wire between the two electrodes is 200 cm;
[0033] S3: Power on: A 40A AC current is applied to the molybdenum alloy wire in the middle through the conductive electrode. At this time, the AC voltage is 5.5V. The wire in the middle gradually becomes red hot and reaches 900°C after about 17 seconds.
[0034] S4: Continuous drawing: Start the wire drawing equipment and draw at a speed of 10cm / s. After the wire enters the contact range of the conductive electrode, it enters the wire drawing die about 18s later. At this time, the temperature has reached 900℃ and it passes through the φ0.95mm wire drawing die smoothly at this temperature. The pass processing rate reaches 9.75%, and the heating power is 220W.
[0035] Example 3
[0036] A high temperature continuous drawing method for refractory brittle metal wire, the specific steps comprising:
[0037] S1: Die insertion: Make a φ0.80mm iridium wire into a drawing head with a length of 10cm and a wire diameter of φ0.70mm~0.75mm, pass it through a φ0.75mm drawing die coated with high-temperature lubricant, and clamp the drawing head with wire clamps;
[0038] S2: Clamping: Use carbide conductive blocks to contact the two ends of the iridium wire. One electrode is located between the wire drawing die and the wire clamp, 5 cm away from the wire drawing die, and the other electrode is located on the other side of the wire drawing die, 45 cm away from the wire drawing die. At this time, the length of the iridium wire between the two electrodes is 50 cm;
[0039] S3: Power on: A 37A DC current is applied to the middle iridium wire through the conductive electrode. At this time, the DC voltage is 1.96V. The middle wire gradually becomes red hot and reaches 810℃ after about 9s.
[0040] S4: Continuous drawing: Start the wire drawing equipment and draw at a speed of 5cm / s. After the iridium wire enters the contact range of the conductive electrode, it enters the wire drawing die about 9s later. At this time, the temperature has reached 810℃ and it passes through the φ0.75mm wire drawing die smoothly at this temperature. The processing rate of each pass reaches 12.11% and the heating power is 72.5W.
[0041] From the above processing examples, it can be seen that the use of this method for high-temperature continuous drawing of refractory brittle metal wires can achieve a higher pass processing rate with extremely low energy consumption. Compared with the power of several kW or even more than ten kW of tubular furnaces, it can significantly reduce processing energy consumption and achieve the effect of reducing costs and increasing efficiency.
[0042] Although embodiments of the present invention have been shown and described (see the above detailed description for details), it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high temperature continuous drawing method for refractory brittle metal wires, Features: Conductive electrodes are used to contact the wires passing through the wire drawing die on both sides, and low voltage and high current are passed through the wire drawing die to make the wires pass through the wire drawing die in a red hot state. The method specifically includes the following steps: S1: Die insertion: Make the head of the refractory brittle metal wire into a wire drawing head, pass it through the wire drawing die coated with high-temperature lubricant, and clamp the wire drawing head with wire clamps; S2: Clamping: using conductive electrodes to contact the two ends of the refractory brittle metal wire respectively; S3: Power on; low voltage and high current are applied to the metal wire in the middle through the conductive electrode, so that the wire in the middle becomes red hot and reaches the temperature required for hot drawing; S4: Continuous drawing: Start the wire drawing equipment and adjust the appropriate speed so that the wire can quickly and continuously reach a red-hot state after entering the contact range of the conductive electrode and before entering the wire drawing die, and the red-hot wire passes through the wire drawing die continuously.
2. A high temperature continuous drawing method for refractory brittle metal wire according to claim 1, Features: The wire drawing head has a taper, and its diameter is smaller than the metal wire body, can pass through the wire drawing die, can be clamped by the wire clamp, and leaves a length margin sufficient for placing the conductive electrode between the wire drawing die and the wire clamp.
3. A high temperature continuous drawing method for refractory brittle metal wire according to claim 1, Features: The conductive electrode is a cylindrical conductive block or a conductive roller, which is provided with a tension device so that the wire can be in close contact with the conductive electrode.
4. A high temperature continuous drawing method for refractory brittle metal wire according to claim 3, Features: The cylindrical conductive block is made of one of hard alloy, beryllium bronze and wear-resistant graphite.
5. A high temperature continuous drawing method for refractory brittle metal wire according to claim 3, Features: The conductive roller is one of a copper conductive roller, a steel conductive roller and a graphite conductive roller.
6. A high temperature continuous drawing method for refractory brittle metal wire according to claim 1, Features: One electrode of the conductive electrode contacts the metal wire that has not entered the wire drawing die, and the other electrode contacts the metal wire between the wire drawing die and the wire clamp. The distance between the two electrodes is determined according to the drawing speed and the actual required heating time.
7. A high temperature continuous drawing method for refractory brittle metal wire according to claim 1, Features: The low voltage and high current is low voltage direct current or low voltage alternating current, and the current value is determined according to the wire diameter, the distance between the two electrodes and the plastic-brittle transition temperature of the metal.