Accurate forming method of thin-wall component with built-in reinforcing blocks

Through the method of using preforming and final forming, prefabricated reinforced bulk cells and inert gas control is used to solve the skin groove problem caused by reinforced blocks in SPF/DB manufacturing, and the forming accuracy and quality of the components are improved, so as to achieve High-quality built-in reinforced block thin-walled components are manufactured.

CN119057225AActive Publication Date: 2024-12-03SHENYANG AIRCRAFT CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411217719.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-03
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

During the manufacturing process of superplastic forming/diffusion connection (SPF/DB), the built-in reinforcement block causes grooves to appear on the outer surface of the skin, affecting the forming quality and performance of the components. The gaps at the reinforcement block are prone to appear during diffusion connection, affecting the impact of the gaps at the reinforcement blocks. Overall forming quality.

Method used

The method of using preforming and final forming is adopted to achieve accurate fit and uniform forming of the reinforced block and skin through the thermoforming tooling design and inert gas control of prefabricated reinforced block cells, thereby inhibiting the occurrence of groove defects.

Benefits of technology

The welding rate and mass consistency between the reinforcement block and the skin are improved, the defects of the rest and groove shrinkage of the components are reduced, and the overall forming quality and service performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057225A_ABST
    Figure CN119057225A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of plastic forming of metal thin-wall components, and relates to a precise forming method of a thin-wall component with built-in reinforcing blocks. According to the method, the pre-forming process and the final forming process are cooperatively used, hot forming is conducted firstly to complete manufacturing of the prefabricated rib cells, then the SPF / DB process is conducted to complete manufacturing of the final component, the existence of the pre-formed rib cells improves the fixing stability of the reinforcing blocks, the welding rate of diffusion connection between the reinforcing blocks and the skin and the consistency of quality are improved, and the product quality is improved. By controlling the protruding height and size of the placed reinforcing block, the final collapse and groove shrinkage defects of the component are restrained, and the overall forming quality of the component is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of plastic forming of metal thin-walled components and relates to a precise forming method of a thin-walled component with a built-in reinforcement block. Background Art

[0002] Superplastic forming / diffusion bonding (SPF / DB) formed components with lightweight and high strength characteristics have been widely used in the manufacturing field of vehicle components. With the development of vehicle design and manufacturing technology, vehicles suitable for multi-scenario use have become the main development trend, and also pose new challenges to the design and manufacturing of new vehicles. Structural parts with gradient characteristics have good adaptability to complex and variable working conditions, and have gradually become one of the important choices for lightweight and high-strength components. The introduction of thin-walled structures with built-in reinforcement blocks has achieved the perfect coupling of lightweight and high-strength characteristics in the manufacturing of thin-walled structures, greatly expanded the application field of SPF / DB technology, and also improved the adaptability of thin-walled components to complex service environments. At present, the main process flow of the thin-walled structure with built-in reinforcement blocks is to fix the reinforcement blocks and the skin by spot welding on the inner surface of the inner skin, then spray the solder stop in the non-diffusion area and seal the outer skin and the inner skin at the edge by welding, and finally, put them into the SPF / DB forming equipment to complete the manufacturing of the components. With this method, due to the presence of built-in reinforcement blocks, a large gap will appear at the built-in reinforcement blocks in the unformed structure that has completed the welding seal. During diffusion connection, the gap is affected by external pressure, and the inner and outer skins are fitted to the middle. However, due to the rigidity of the reinforcement blocks, the amount of skin fitting at the reinforcement blocks is much smaller than that without reinforcement blocks. The difference between the two eventually leads to grooves on the outer surface of the skin, affecting the overall forming quality of the structure. The grooves form a large stress concentration during use, which reduces the performance of the product. Therefore, it is urgent to find a more suitable SPF / DB forming method for thin-walled components with built-in reinforcement blocks to solve existing problems in production and improve quality and efficiency. Summary of the invention

[0003] In view of the problem that defects are prone to occur in the traditional SPF / DB manufacturing process mentioned above, a precise forming method for thin-walled components with built-in reinforcement blocks is proposed. The present invention adopts a method of coordinated use of preforming and final forming, and controls the process of preforming and final forming respectively, so as to improve the forming efficiency, quality and precision of the components. Preforming refers to prefabricating a rib cell depression in the placement area of ​​the reinforcement block in the flat state. By reasonably designing the configuration of the preforming mold and controlling the depth and outer dimensions of the prefabricated rib cell, the relative position of the reinforcement block and the plate is positioned, and the position accuracy of the diffusion connection of the reinforcement block is improved. At the same time, the separation of the reinforcement block and the skin before diffusion connection improves the quality consistency of the reinforcement block and the skin after diffusion forming; final forming refers to the introduction of three inert gases into the fitting surfaces of the inner and outer skin surfaces and the mold and the reinforcement cell during SPF / DB forming, and adjusting the inert gas flow at the reinforcement rib package and the fitting surfaces of the two skins and the tooling respectively, controlling the gas pressure on the fitting surfaces of the skin and the tooling and the reinforcement rib package, as well as the on-off of each gas path, guiding the flow direction and flow behavior of the metal during superplastic forming, improving the stability of superplastic forming, suppressing the groove defects on the outer surface of the component, and finally achieving high-quality SPF / DB forming of thin-walled components with built-in reinforcement blocks.

[0004] The technical means adopted by the present invention are as follows:

[0005] The method for accurately forming a thin-walled component with an internal reinforcement block is characterized in that, first, a hot forming tool for prefabricated rib cells is designed according to the size of the internal reinforcement block and the specification of the thin-wall skin, and an SPF / DB final forming tool is designed according to the final shape requirements of the component; in the second step, after the prefabricated rib cells are formed, the reinforcement blocks are placed at the prefabricated rib cells, the coating area of ​​the solder stop is determined and the coating of the solder stop is completed; in the third step, laser welding and sealing of the cavities of the inner and outer skins of the component before superplastic forming are completed to form a prefabricated integral part; in the fourth step, the formed prefabricated integral part is placed in the SPF / DB final forming tool and fixed to the SPF / DB forming equipment, each control gas path is connected, the gas flow rate and the on and off of the air flow of each path are controlled, and the SPF / DB forming of the final component is completed.

[0006] 1. Determination of the specifications of the prefabricated reinforcement block

[0007] The prefabricated reinforcement block rib cell is a part of the reinforcement block rib cell of the final component. The outer contour size of the prefabricated reinforcement block rib cell is determined according to the proposed prefabricated reinforcement block rib cell height H. After the prefabricated reinforcement block rib cell height H is determined, a virtual section is constructed by measuring the height H from the reinforcement block rib cell of the final component with the rib cell protrusion plane as the reference to the skin side. The outer contour of the intercepted segment is the outer contour of the prefabricated reinforcement block rib cell.

[0008] The prefabricated reinforcement block rib cell height H is determined by the reinforcement block thickness c. In order to improve the manufacturing accuracy of the subsequent manufacturing process, the two should satisfy the relationship shown in formula (1):

[0009] c+0.1 mm≤H≤c+0.5 mm (1)

[0010] 2. Design criteria for prefabricated reinforcement block rib cell forming tooling

[0011] The prefabricated reinforcement block rib cell forming tool is a hot forming tool, which is used to preform the reinforcement block rib cell contour based on the flat plate raw material. Its overall configuration is divided into an upper die and a lower die. The forming surface of the upper die is a plane as a whole, and a protrusion is formed at the corresponding position of the simulated reinforcement block rib cell. The forming surface of the lower die is also a plane as a whole, and a depression is formed at the corresponding position of the simulated reinforcement block rib cell. The outer contour size and height of the protrusion and the outer contour size and depth of the depression are determined according to the already determined size of the prefabricated reinforcement block rib cell.

[0012] There should be a chamfer of about R5 at the bottom of the reinforcement cell of the prefabricated reinforcement block to suppress excessive stress concentration at the bottom of the reinforcement cell during the subsequent final component forming;

[0013] 3. Prefabricated reinforcement block cell manufacturing

[0014] The flat sheet is placed in the prefabricated reinforcement block forming tooling, and the prefabricated reinforcement block rib cell is formed by a hot forming process. Then, the reinforcement block is placed in the prefabricated reinforcement block rib cell, and the reinforcement block is ensured to be about 0.1 to 0.5 mm lower than the rib cell height, so as to facilitate the fixing of the reinforcement block during subsequent forming. A solder stopper is applied on the upper surface of the reinforcement block, and the outer skin is placed above the prefabricated reinforcement block rib cell skin. The inner and outer skins are sealed and welded by laser welding in an external corner joint manner to form a prefabricated integral part.

[0015] 4. SPF / DB forming of integral components

[0016] (1) Place the prefabricated integral part that has completed sealing welding on the SPF / DB forming tooling and then load it into the forming furnace together, complete the inert gas path connection between the reinforcement block rib package and the two skins and the tooling bonding surface, first extract from the reinforcement block rib cell to complete the close bonding of the inner surface of the skin, and increase the furnace temperature to complete the diffusion connection between the reinforcement block of the prefabricated integral part and the inner skin and the skin bonding area except the prefabricated rib cell;

[0017] (2) Inert gas is filled into the prefabricated rib cells and the gap between the outer surface of the rib cells and the cavity, and the inert gas flow rate is adjusted to control the pressure of the two inert gases during the forming process. Under the action of the inert gas pressure, the forming of the reinforcement block rib cells is completed. The forming process should be carried out at a uniform rate to avoid excessive forming rate, which will lead to instability of the formed thin wall and eventually cause tearing defects;

[0018] (3) After the superplastic forming process of the component is completed, inert gas is introduced into the reinforcement block and the joint surface between the two skins and the tooling to ensure a certain pressure until the straight component cools to room temperature, so as to avoid the component from being dented due to a sudden drop in gas pressure when the component is in a high temperature state.

[0019] Beneficial effects of the present invention

[0020] The present invention proposes a precise forming method for thin-walled components with built-in reinforcement blocks. The preforming and final forming processes are used in coordination. Hot forming is first performed to complete the manufacture of prefabricated rib cells, and then the SPF / DB process is performed to complete the manufacture of the final component. The presence of the preformed rib cells improves the stability of the reinforcement block fixation, improves the welding rate and quality consistency of the diffusion connection between the reinforcement block and the skin, and suppresses the final sagging and shrinkage defects of the component by controlling the protruding height of the reinforcement block, thereby improving the overall forming quality of the component. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram of a thin-walled component with an internal reinforcement block;

[0022] Figure 2 This is a schematic diagram of prefabricated reinforcement cells;

[0023] Figure 3 To form prefabricated reinforcing rib cells;

[0024] Figure 4 Schematic diagram of prefabricated integral parts;

[0025] Figure 5 Schematic diagram of SPF / DB molding.

[0026] In the figure: 1 is a pneumatic skin panel; 2 is a non-pneumatic skin panel; 3 is an internal reinforcement block; 4 is a prefabricated reinforcement block rib cell; 5 is a rib cell protrusion plane; 6 is a virtual section; 7 is a corner of the bottom of the rib cell; 8 is an upper die of a forming tool for prefabricated reinforcement block rib cells; 9 is a lower die of a forming tool for prefabricated reinforcement block rib cells; 10 is a protrusion of an upper die of a forming tool for prefabricated reinforcement block rib cells; 11 is a depression of an upper die of a forming tool for prefabricated reinforcement block rib cells; 12 is an outer skin; 13 is a prefabricated integral part; 14 is an SPF / DB forming tool upper die; 15 is an SPF / DB forming tool lower die. DETAILED DESCRIPTION

[0027] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings. The following embodiments are used to illustrate the present invention but are not used to limit the scope of application of the present invention.

[0028] Thin-walled components with built-in reinforcement blocks such as Figure 1 As shown, its overall structure consists of three parts: a pneumatic skin panel 1, a non-pneumatic skin panel 2 and a built-in reinforcement block 3. The specific forming and manufacturing steps are divided into the following steps:

[0029] Step 1: Determine the specifications of the prefabricated reinforcement block

[0030] The digital model of the simulated component is opened in the 3D drawing software. The thickness c of the reinforcement block 3 is measured to be 8 mm. According to formula (1), the height H of the prefabricated reinforcement block rib cell 4 is calculated to be 8.1-8.5 mm. 8.5 mm is selected as the height. In the digital model of the component, a virtual section 6 is constructed based on the rib cell protrusion plane 5. At this time, the outer contour of the segmented body is the outer contour of the prefabricated reinforcement block rib cell 4, and the corner 7 at the bottom of the prefabricated reinforcement block rib cell needs to be preset as the chamfer of R5.

[0031] Step 2: Design of prefabricated reinforcement block rib cell forming tooling

[0032] The forming tooling of the prefabricated reinforcement block rib cell is divided into two parts: an upper die 8 and a lower die 9. The forming surface of the upper die 8 is provided with a protrusion 10 consistent with the profile of the prefabricated reinforcement block at a corresponding position of the cell of the simulated reinforcement block, and the forming surface of the lower die 9 is provided with a depression 11 consistent with the profile of the prefabricated reinforcement block at a corresponding position of the cell of the simulated reinforcement block.

[0033] Step 3: Prefabricated reinforcement cell manufacturing

[0034] The flat sheet is placed in the prefabricated reinforcement block forming tooling, and the prefabricated reinforcement block rib cell 4 is formed by a hot forming process. Then, the reinforcement block 3 is placed in the prefabricated reinforcement block rib cell, ensuring that the reinforcement block is about 0.1 to 0.5 mm lower than the rib cell height, and a solder stop is applied on the upper surface of the reinforcement block 3. The outer skin 12 is placed above the prefabricated reinforcement block rib cell skin, and the inner and outer skins are sealed and welded by laser welding in an external corner joint manner to form a prefabricated integral part 13;

[0035] Step 4: SPF / DB forming of the whole component

[0036] (1) The prefabricated integral part 13 after the sealing welding is placed between the upper die 14 of the SPF / DB forming tool and the lower die 15 of the SPF / DB forming tool, and loaded into the forming furnace together, and the inert gas path connection between the reinforcement block rib package and the two skins and the tooling bonding surface is completed. First, it is extracted from the reinforcement block rib cell to complete the close fitting of the inner surface of the skin, and the furnace temperature is increased to complete the diffusion connection between the reinforcement block of the prefabricated integral part and the inner skin and the skin bonding area except the prefabricated rib cell;

[0037] (2) Inert gas is filled into the prefabricated rib cells and the gap between the outer surface of the rib cells and the cavity, and the inert gas flow rate is adjusted to control the pressure of the inert gas on both sides during the forming process. Under the action of the inert gas pressure, the forming of the reinforcement block rib cells is completed. The forming process should be carried out at a uniform rate to avoid the forming rate being too fast, which will cause the thin wall to be unstable under stress and eventually produce tearing defects;

[0038] (3) After the superplastic forming process of the component is completed, inert gas is introduced into the reinforcement block and the joint surface between the two skins and the tooling to ensure a certain pressure until the straight component cools to room temperature, so as to avoid the component from being dented due to a sudden drop in gas pressure when the component is in a high temperature state.

Claims

1. A method for accurately forming a thin-walled component with a built-in reinforcement block, characterized in that: Here are the steps: Step 1: Design the prefabricated reinforcement block rib cell forming tooling according to the size of the built-in reinforcement block and the specifications of the thin-wall skin, and design the SPF / DB final forming tooling according to the final shape requirements of the component; Step 2: After the prefabricated rib cell is formed, the reinforcement block is placed at the prefabricated rib cell, the solder stop coating area is determined and the solder stop coating is completed; Step 3: Complete the laser welding and sealing of the cavities of the inner and outer skins before superplastic forming of the component to form a prefabricated integral component; The fourth step is to place the formed prefabricated integral part in the SPF / DB final forming tooling and fix it to the SPF / DB forming equipment, connect each control gas path, control the incoming gas flow and the on and off of the air flow in each path, and complete the SPF / DB forming of the final component.

2. The method for accurately forming a thin-walled component with an internal reinforcement block according to claim 1, characterized in that: In the first step, the specifications of the prefabricated reinforcement block reinforcement cells are determined as follows: The prefabricated reinforcement block rib cell is a part of the reinforcement block rib cell of the final component. The outer contour size of the prefabricated reinforcement block rib cell is determined according to the proposed prefabricated reinforcement block rib cell height H. After the prefabricated reinforcement block rib cell height H is determined, a virtual section is constructed by measuring the height H at the reinforcement block rib cell of the final component with the rib cell protrusion plane as the reference to the skin side. The outer contour of the intercepted segment is the outer contour of the prefabricated reinforcement block rib cell. The prefabricated reinforcement block rib cell height H is determined by the thickness c of the reinforcement block, and the two should satisfy the relationship shown in formula (1): c+0.1 mm≤H≤c+0.5 mm (1).

3. The method for accurately forming a thin-walled component with an internal reinforcement block according to claim 1 or 2, characterized in that: In the first step, the prefabricated reinforcement block rib cell forming tool is a hot forming tool, and its overall configuration is divided into an upper die and a lower die. The forming surface of the upper die is a plane as a whole, and a protrusion is formed at the corresponding position of the simulated reinforcement block rib cell. The forming surface of the lower die is also a plane as a whole, and a depression is formed at the corresponding position of the simulated reinforcement block rib cell. The outer contour size and height of the protrusion and the outer contour size and depth of the depression are determined according to the determined size of the prefabricated reinforcement block rib cell. There should be a chamfer of about R5 at the bottom of the prefabricated reinforcement block rib cell to suppress excessive stress concentration at the bottom of the rib cell during subsequent final component forming.

4. The method for accurately forming a thin-walled component with an internal reinforcement block according to claim 1 or 2, characterized in that: The manufacturing method of the prefabricated reinforcement block rib cell is as follows: The flat sheet is placed into the prefabricated reinforcement block forming tooling, and the prefabricated reinforcement block rib cell is formed by a hot forming process. Then, the reinforcement block is placed in the prefabricated reinforcement block rib cell, ensuring that the reinforcement block is about 0.1 to 0.5 mm lower than the rib cell height, so as to fix the reinforcement block during subsequent forming. A solder stopper is applied on the upper surface of the reinforcement block, and the outer skin is placed above the prefabricated reinforcement block rib cell skin. The inner and outer skins are sealed and welded by laser welding using an external corner joint method to form a prefabricated integral part.

5. The method for accurately forming a thin-walled component with an internal reinforcement block according to claim 3, characterized in that: The manufacturing method of the prefabricated reinforcement block rib cell is as follows: The flat sheet is placed into the prefabricated reinforcement block forming tooling, and the prefabricated reinforcement block rib cell is formed by a hot forming process. Then, the reinforcement block is placed in the prefabricated reinforcement block rib cell, ensuring that the reinforcement block is about 0.1 to 0.5 mm lower than the rib cell height, so as to fix the reinforcement block during subsequent forming. A solder stopper is applied on the upper surface of the reinforcement block, and the outer skin is placed above the prefabricated reinforcement block rib cell skin. The inner and outer skins are sealed and welded by laser welding using an external corner joint method to form a prefabricated integral part.

6. The method for accurately forming a thin-walled component with an internal reinforcement block according to claim 1, 2 or 5, characterized in that: The SPF / DB forming method is as follows: (1) Place the prefabricated integral part that has completed sealing welding on the SPF / DB forming tooling and then load it into the forming furnace together, complete the inert gas path connection between the reinforcement block rib package and the two skins and the tooling bonding surface, first extract from the reinforcement block rib cell to complete the close bonding of the inner surface of the skin, and increase the furnace temperature to complete the diffusion connection between the reinforcement block of the prefabricated integral part and the inner skin and the skin bonding area except the prefabricated rib cell; (2) Inert gas is filled into the prefabricated rib cells and the gap between the outer surface of the rib cells and the cavity, and the flow rate of the inert gas is adjusted to control the pressure of the inert gas on both sides during the forming process; (3) After the superplastic forming process of the component is completed, inert gas is introduced into the reinforcement block and the joint surface between the two skins and the tooling to ensure that the pressure is maintained until the straight component cools to room temperature.

7. The method for accurately forming a thin-walled component with an internal reinforcement block according to claim 3, characterized in that: The SPF / DB forming method is as follows: (1) Place the prefabricated integral part that has completed sealing welding on the SPF / DB forming tooling and then load it into the forming furnace together, complete the inert gas path connection between the reinforcement block rib package and the two skins and the tooling bonding surface, first extract from the reinforcement block rib cell to complete the close bonding of the inner surface of the skin, and increase the furnace temperature to complete the diffusion connection between the reinforcement block of the prefabricated integral part and the inner skin and the skin bonding area except the prefabricated rib cell; (2) Inert gas is filled into the prefabricated rib cells and the gap between the outer surface of the rib cells and the cavity, and the flow rate of the inert gas is adjusted to control the pressure of the inert gas on both sides during the forming process; (3) After the superplastic forming process of the component is completed, inert gas is introduced into the reinforcement block and the joint surface between the two skins and the tooling to ensure that the pressure is maintained until the straight component cools to room temperature.

8. The method for accurately forming a thin-walled component with an internal reinforcement block according to claim 4, characterized in that: The SPF / DB forming method is as follows: (1) Place the prefabricated integral part that has completed sealing welding on the SPF / DB forming tooling and then load it into the forming furnace together, complete the inert gas path connection between the reinforcement block rib package and the two skins and the tooling bonding surface, first extract from the reinforcement block rib cell to complete the close bonding of the inner surface of the skin, and increase the furnace temperature to complete the diffusion connection between the reinforcement block of the prefabricated integral part and the inner skin and the skin bonding area except the prefabricated rib cell; (2) Inert gas is filled into the prefabricated rib cells and the gap between the outer surface of the rib cells and the cavity, and the flow rate of the inert gas is adjusted to control the pressure of the inert gas on both sides during the forming process; (3) After the superplastic forming process of the component is completed, inert gas is introduced into the reinforcement block and the joint surface between the two skins and the tooling to ensure that the pressure is maintained until the straight component cools to room temperature.

Citation Information

Patent Citations

  • Super-plastic forming / diffusion bonding forming method for large-curvature complex surface titanium alloy part

    CN104588982A

  • Integral forming method for titanium alloy skin with reinforcing rib structure

    CN105149874A

  • Superplastic forming diffusion connection integral forming mold and method for parts with reinforcing ribs

    CN106270095A

  • Large-depth-diameter-ratio rotation thin-wall titanium alloy component and forming method thereof

    CN111774487A

  • Integrated forming method for titanium alloy skin with mounting part