Novel stand column jack connector welding system
Through the self-repair design of the limit liquid column and sealing ring, the problem of cumbersome welding process and liquid leakage of jack joints is solved, the production efficiency and product reliability are improved, and the service life is extended.
Patent Information
- Application Number
- CN202411401580.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-03
AI Technical Summary
The welding process of existing mining hydraulic jack joints is complicated and time-consuming, and it is prone to welding defects and liquid leakage, resulting in low production efficiency and poor product reliability.
The limit-liquid column design is adopted, and the joints and cylinders are connected through limit-liquid columns. The self-healing function of the sealing ring and the non-cylindrical design are used to reduce welding steps and sealing gaps, and positioning accuracy and sealing performance are improved.
The processing process is simplified, welding accuracy and reliability are improved, welding defects are reduced, product life is extended, production costs are reduced, and overall structural strength and sealing performance are improved.
Smart Images

Figure CN119057295A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of jacks, and in particular relates to a novel column jack joint welding system. Background Art
[0002] The joints for connecting the hydraulic pipes of mining hydraulic jacks are usually welded all around the cylinder body. The vertical liquid hole from the joint to the cylinder body is usually opened, then welded to the cylinder body, and then transferred to the drilling machine to drill through the cylinder body along the joint hole, and finally transferred to the welding workshop to weld the upper end of the joint hole. Figure 1-2 As shown, the joint A of the prior art is welded on the cylinder body C. There is a liquid hole B on the joint A. The liquid hole B is T-shaped. After the joint A is welded to the cylinder body C, the liquid hole in the vertical direction of the cylinder body C is opened to form a liquid hole D on the cylinder body. The joint A is welded to the cylinder body C by electric welding to form a welding point E. Then, the upper end of the joint hole is welded to form a plugged weld F. The processing procedures of this structure of the prior art are cumbersome, the back and forth sequence time is long, and a large amount of production cycle is wasted. In addition, since the joint and the cylinder body are in surface contact, the joint position of the liquid hole and the liquid hole is not protected, causing the liquid to be pressed onto the weld from the joint position of the cylinder body liquid hole and the joint liquid hole along the gap of the contact surface when the liquid is passed and pressurized. In addition, it is difficult for workers to position the joint when welding. They need to mark and position one by one, and it is easy to weld crooked. In addition, welding defects are easily formed after the joint is welded. After the pressure test, liquid often flies out from the joint welding position between the cylinder body and the joint. Summary of the invention
[0003] The purpose of the present invention is to provide a novel column jack joint welding system to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] A novel column jack joint welding system includes a cylinder body, a joint is fixedly provided on the outer wall of the cylinder body, a joint liquid hole is provided inside the joint, a cylinder liquid hole is provided on the cylinder body, the joint liquid hole and the cylinder liquid hole are connected by a limiting liquid column, a limiting column liquid hole is penetrated inside the limiting liquid column, and the limiting column liquid hole connects the joint liquid hole and the cylinder liquid hole.
[0006] Furthermore, the outer wall of the limiting liquid column is provided with a plurality of annular grooves, and matching sealing rings are installed in the grooves, and limiting blocks are provided at both ends of the sealing rings.
[0007] Furthermore, the fluid passage hole of the joint is L-shaped.
[0008] Furthermore, an installation groove a is provided at one end of the joint liquid hole close to the cylinder body, and an installation groove b corresponding to the installation groove a is provided at one end of the cylinder body liquid hole close to the joint, and the two ends of the limiting liquid column are correspondingly installed in the installation groove a and the installation groove b.
[0009] Furthermore, the outer contour of the limiting liquid column is a non-cylindrical column, and the installation groove a and the installation groove b for installing the limiting liquid column are installation grooves that match the outer contour of the limiting liquid column, and the limiting column liquid hole is a circular hole that is compatible with the joint liquid hole and the cylinder liquid hole.
[0010] Furthermore, the outer contour of the limiting liquid column is an elliptical cylinder, and the mounting groove b on the outer side of the cylinder body liquid hole and the mounting groove a at the lower end of the joint liquid hole are corresponding elliptical mounting grooves.
[0011] Furthermore, the sealing ring includes an inner ring and an outer ring, wherein the inner ring is rubber and the outer ring is a microcapsule composite material, and the inner ring and the outer ring are combined by coating the microcapsule composite colloid on the surface of the rubber ring, coating the second layer of microcapsule composite colloid after the first layer of microcapsule composite colloid is cured, coating the third layer of microcapsule composite colloid after the second layer of microcapsule composite colloid is cured, and the cycle is repeated until the size requirements are met. Furthermore, the preparation method of the rubber ring includes: firstly plasticizing the fluororubber, then gradually adding sulfur, accelerator, activator, anti-scorch agent, carbon black, paraffin oil, and antioxidant RD, uniformly dispersing the components in the rubber matrix for mixing, and then placing the mixed rubber into a vulcanization device for vulcanization treatment, and after the vulcanization is completed, cooling the rubber ring to room temperature to obtain the rubber ring.
[0012] Further, the weight ratio of each component of the rubber ring is:
[0013] Fluororubber: 100 parts;
[0014] Sulfur: 1-2 parts;
[0015] Accelerator: 1.5-2 parts;
[0016] Activator: 2-5 parts;
[0017] Anti-scorching agent: 0.5-1 part;
[0018] Carbon black: 50-55 parts;
[0019] Paraffin oil: 10-15 parts;
[0020] Anti-aging agent RD: 1-2 parts.
[0021] Furthermore, the preparation method of the microcapsule composite colloid includes: dissolving polyester in a solvent to form an emulsion, adding an epoxy resin repair agent to the emulsion, and then forming microcapsules of the polyester around the epoxy resin repair agent through interfacial polymerization or in situ polymerization; mixing the polyurethane matrix and the curing agent evenly, and then adding microcapsules, glass fibers, leveling agents and defoaming agents, and continuing to stir until evenly dispersed to obtain a microcapsule composite colloid.
[0022] The beneficial effects of this application are specifically reflected in the following aspects:
[0023] Simplify the processing steps: Traditional processing methods require multiple transfer steps, including welding, drilling, and re-welding. The technical solution of the present application uses the design of a limited liquid column so that the connection between the joint and the cylinder body can be installed after one assembly, reducing the cumbersome transfer steps and saving a lot of production time.
[0024] Reduce processing time: There is no need to repeatedly transfer workpieces between different processes, which reduces handling time and waiting time and improves overall production efficiency.
[0025] Improve welding accuracy and reliability
[0026] Automatic positioning: The joint can be automatically positioned by the guiding effect of the limit liquid column, without the need for manual marking, reducing human errors and improving welding accuracy.
[0027] Reduce welding defects: The design of limiting the liquid column avoids the problem of welding deviation that is easy to occur in traditional welding methods. At the same time, it reduces the possibility of liquid directly acting on the weld during welding, thereby reducing the probability of welding defects.
[0028] Improve sealing performance
[0029] Self-repair function: The sealing ring is designed with a composite material of inner ring rubber and outer ring microcapsule. When the sealing ring is damaged, the microcapsules rupture and release the repair agent to achieve self-repair function, thereby maintaining good sealing performance.
[0030] Multiple protections: There are limit blocks at both ends of the sealing ring, which can provide additional support under high pressure to prevent the sealing ring from deforming and further enhance the sealing effect.
[0031] Extend service life
[0032] Reduce welds: No additional welding is required between the joint and the cylinder body, which reduces the number of welds, reduces the potential failure risk caused by welds, and extends the service life of the hydraulic system.
[0033] Improve structural strength: By optimizing the design and reducing unnecessary welding steps, the strength of the overall structure is improved, thereby increasing the reliability and life of the hydraulic system.
[0034] Comprehensive Benefits
[0035] Cost saving: A series of improvement measures such as reducing processes, improving precision, and reducing failure rates can help reduce production and maintenance costs and improve economic benefits.
[0036] Improve product quality: By optimizing design and improving production efficiency, high-quality product output is ensured and market competitiveness is enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a radial cross-sectional view of the outer cylinder joint of the existing jack;
[0038] Figure 2 It is an axial cross-sectional view of the outer cylinder joint of the existing jack;
[0039] Figure 3 It is an axial cross-sectional view of the outer cylinder joint of the present invention;
[0040] Figure 4 It is a top view of the limited liquid column of the present invention;
[0041] Figure 5 This is an axial cross-sectional view of the limited liquid column of the present invention;
[0042] Figure 6 It is an axial cross-sectional view of the outer cylinder body of the present invention;
[0043] Figure 7 It is an axial cross-sectional view of the joint of the present invention;
[0044] In the figure:
[0045] 1. Joint, 2. Joint liquid hole, 3. Cylinder body, 3-1. Cylinder body liquid hole, 4. Limit block, 5. Sealing ring, 6. Limit liquid column, 7. Limit column liquid hole, 8. Solder point, 9. Blocking weld, 10. Installation groove a, 11. Installation groove b, 12. Groove. DETAILED DESCRIPTION
[0046] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] The invention is suitable for a column jack with a thick cylinder body.
[0048] The present invention provides a novel column jack joint welding system, such as Figures 3 to 7, including a cylinder body 3, the outer side of the cylinder body liquid hole 3-1 on the cylinder body 3 is processed into an elliptical installation groove b11, the lower end of the joint liquid hole 2 of the joint 1 is processed into an elliptical installation groove a10, the sealing ring 5 is installed in the groove 12 of the outer wall of the limit liquid column 6, the limit blocks 4 are respectively placed at both ends of the corresponding sealing ring 5, the limit blocks 4 play a supporting role to prevent the seal from deforming under high pressure, the assembled limit liquid column 6 is inserted into the installation groove a10 and the installation groove b11, at this time the position of the joint 1 is just in the installation position, the installation groove b10 opened on the cylinder body 3 11 is opened in the same direction as the elliptical hole of the installation groove a10 opened at the lower end of the joint liquid hole 2. After installation, the limiting column liquid hole 7 is perpendicular to the cylinder mouth direction of the cylinder body 3. A penetrating limiting column liquid hole 7 is opened in the middle of the limiting liquid column 6. The limiting column liquid hole 7 is a circular hole compatible with the joint liquid hole 2 and the cylinder body liquid hole 3-1. After installation, the joint liquid hole 2 close to the cylinder body 3, the cylinder body liquid hole 3-1 and the limiting column liquid hole 7 on the limiting liquid column 6 are in a straight line. A welding machine is used to weld the joint 1 and the cylinder body 3 in a circle to fix it.
[0049] In a preferred embodiment, Figure 4 As shown, the outer contour of the limiting liquid column 6 is an elliptical cylinder, and the mounting groove b11 outside the cylinder liquid hole 3-1 and the mounting groove a10 at the lower end of the joint liquid hole 2 are corresponding elliptical mounting grooves.
[0050] In other embodiments, the shape of the limiting liquid column 6 can be a non-cylindrical column of any other shape, including but not limited to square, hexagonal or polygonal shapes. These different shape designs can be selected according to the needs of the actual application scenario, such as to better adapt to specific space limitations or to enhance the mechanical strength in certain specific directions. Regardless of the shape, the shapes of the mounting groove a10 and the mounting groove b11 should match the outer contour of the limiting liquid column 6 to ensure that the limiting liquid column 6 can be accurately installed in place and can effectively transfer liquid while ensuring the sealing between the joint 1 and the cylinder body 3. Including, if a square column is selected as the shape of the limiting liquid column 6, then the mounting groove a10 and the mounting groove b11 also need to be designed as corresponding square grooves. Such a design can not only ensure the correct direction of the limiting liquid column 6 during installation, but also increase the contact area and improve the overall stability and compressive resistance of the structure. At the same time, the design of the square column is also conducive to more accurate positioning during the installation process and reduces errors caused by manual operation. For the hexagonal or polygonal column design, the principle is similar to that of the square column, and the main purpose is to improve the convenience of installation and the stability of the structure. The polygonal design can also provide more variant options to cope with more complex usage environments. Regardless of which non-cylindrical column shape is adopted, the inner part of the limiting liquid column 6 must retain the limiting column liquid hole 7 that passes through to ensure the normal circulation of the liquid. In addition, the design of the groove 12 on the outer wall of the limiting liquid column 6 and the sealing ring 5 installed therein should also be adjusted accordingly to ensure the sealing effect under different shapes. In summary, although there are many options for the shape of the limiting liquid column 6, its core design principle is to ensure that the connection between the joint 1 and the cylinder body 3 is both convenient and firm, while ensuring good sealing performance.
[0051] The present invention can effectively improve production efficiency, and can be installed and formed after one assembly, without the need to rotate the same position of the technicians back and forth. At the same time, it can effectively reduce the leakage of welding defects caused by the high-pressure liquid directly acting on the welding position, and only needs to ensure the welding strength. The present invention is convenient for welding, and only needs to be processed and formed once during processing. When welding, the insertion joint direction is automatically installed in place, and there is no need to mark and position, which saves a lot of working time and has a high accuracy rate. In addition, the joint does not need to be welded and blocked, which not only saves labor and effort, but also reduces welds, ensures the strength of the hydraulic cylinder, and extends the service life.
[0052] In actual production, ordinary rubber sealing rings may crack or be damaged for a long time due to hydraulic shock or high temperature and high pressure. When high-pressure liquid is passed, liquid may still enter the outer wall of the limit liquid column 6 from the joint liquid hole 2, and then penetrate into the docking position between the joint 1 and the cylinder body 3 and apply pressure to the weld along the gap of the contact surface. Therefore, the present application also proposes to improve the sealing ring 5, and the specific solution is as follows:
[0053] The sealing ring 5 comprises an inner ring and an outer ring, wherein the inner ring is a rubber ring and the outer ring is a microcapsule composite ring;
[0054] The rubber ring is composed of the following raw materials in parts by weight:
[0055] Fluororubber (FKM): 100 parts
[0056] Fluororubber is an ideal base material choice due to its excellent heat and oil resistance.
[0057] Sulfur (S): 2-3 parts
[0058] Used in the vulcanization of fluororubber to form a cross-linked structure and improve the mechanical properties of the rubber.
[0059] Accelerator (such as CBS or DM): 1-2 parts
[0060] CBS (dithiocarbamate) or DM (morpholine disulfide) is used to accelerate the vulcanization reaction and shorten the vulcanization time.
[0061] Activator (such as zinc stearate): 2-3 parts
[0062] Zinc stearate can act as an activator to help the accelerator work better.
[0063] Anti-scorch agent (such as NS): 0.5-1 part
[0064] NS (N-cyclohexyl-2-benzothiazole sulfenamide) is used to prevent premature vulcanization, i.e., to prevent scorch.
[0065] Carbon black (N330 or N550): 50-70 parts
[0066] Carbon black, as a reinforcing filler, can significantly improve the hardness and wear resistance of rubber rings.
[0067] Paraffin oil: 10-20 parts
[0068] Paraffin oil acts as a softener and helps improve the processing properties of rubber.
[0069] Antioxidant RD (or 4010NA): 1-2 parts
[0070] Antiaging agents are used to improve the anti-aging properties of rubber and extend its service life.
[0071] The preparation method comprises the steps of:
[0072] Put the fluororubber into the internal mixer for plasticization to achieve a certain plasticity, gradually add sulfur, accelerator, activator, anti-scorch agent, carbon black, paraffin oil, antioxidant RD, etc. to ensure that each component is evenly dispersed in the rubber matrix, put the mixed rubber into the vulcanization equipment, and vulcanize it at a certain temperature (such as 170-200℃) and pressure to form a rubber ring with high elasticity and good wear resistance. After vulcanization, cool the rubber ring to room temperature and carry out necessary size and appearance inspections to ensure that the product meets quality requirements.
[0073] The microcapsule colloid is composed of the following raw materials in parts by weight:
[0074] Base material: 100 parts of polyurethane (PU). Polyurethane is used as the base material and has good elasticity and wear resistance.
[0075] 10-20 parts of microcapsules. The shell of the microcapsules is polyester. The shell contains a repairing agent (such as epoxy resin). When damaged, the shell ruptures to release the repairing agent to fill the cracks.
[0076] 10-15 parts of phenol A type epoxy curing agent, the epoxy curing agent is used to react with polyurethane to form a stable cross-linking structure and improve the mechanical properties of the composite ring.
[0077] Reinforcement material: 50-60 parts of glass fiber. Glass fiber as a reinforcement material can significantly improve the strength and toughness of the composite ring.
[0078] 1-2 parts of leveling agent. The leveling agent is used to improve the flatness of the composite ring surface and reduce bubbles and defects.
[0079] 0.5-1 part of defoaming agent, which is used to eliminate bubbles generated during the preparation process and improve the density of the material.
[0080] The preparation method of the microcapsule composite colloid comprises: dissolving polyester in a solvent to form an emulsion, adding an epoxy resin repair agent into the emulsion, and then forming microcapsules of the polyester around the epoxy resin repair agent through interfacial polymerization or in-situ polymerization; mixing a polyurethane matrix and a curing agent evenly, and then adding microcapsules, glass fibers, a leveling agent and a defoaming agent, and continuing to stir until evenly dispersed to obtain a microcapsule composite colloid.
[0081] The inner ring and the outer ring are combined by coating the microcapsule composite colloid on the surface of the rubber ring, coating the second layer of microcapsule composite colloid after the first layer of microcapsule composite colloid is solidified, coating the third layer of microcapsule composite colloid after the second layer of microcapsule composite colloid is solidified, and the cycle is repeated until the size requirements are met.
[0082] Embodiment, the operation method comprises the steps of:
[0083] Clean the surface of the rubber ring to ensure that there is no impurity such as oil, dust, etc. Use a brush, spray equipment or dip coating to evenly apply the microcapsule composite colloid on the surface of the rubber ring, ensuring that the first layer of colloid covers the entire outer surface of the rubber ring without missing any area. Control the thickness of the first layer of colloid so that it is neither too thin nor too thick to ensure good adhesion of the subsequent layers. After the first layer is applied, place the rubber ring under appropriate temperature and humidity conditions for curing. After the first layer is completely cured, repeat the above coating steps and apply the second layer of microcapsule composite colloid. Also pay attention to thickness control and ensure that the second layer is tightly combined with the first layer. Curing treatment is performed again. Repeat the above coating and curing steps until the required total thickness is reached. After each layer is cured, check for bubbles, cracks or other defects and repair them if necessary. After the last layer is cured, measure the total thickness of the composite ring to ensure that it meets the design requirements. If there is a deviation, the number of coatings can be appropriately increased or decreased to make adjustments. Grind or polish the surface of the composite ring to make it smooth and flat.
[0084] Example 1
[0085] Rubber ring preparation:
[0086] The raw materials include 100 parts of fluororubber (FKM), 2 parts of sulfur (S), 1.5 parts of accelerator (CBS), 2 parts of activator (zinc stearate), 0.5 parts of scorch retarder (NS), 55 parts of carbon black (N550), 15 parts of paraffin oil, and 1 part of antioxidant RD;
[0087] Put the fluororubber into an internal mixer for plasticization, and gradually add sulfur, accelerator, activator, anti-scorch agent, carbon black, paraffin oil, and antioxidant RD to ensure that each component is evenly dispersed in the rubber matrix. Put the mixed rubber into the vulcanization equipment and vulcanize it at 180℃ and 10MPa pressure for 30 minutes. After the vulcanization is completed, cool the rubber ring to room temperature and check its size and appearance.
[0088] Preparation of microcapsule composite colloid:
[0089] The raw materials include 100 parts of polyurethane (PU), 15 parts of microcapsules (containing epoxy resin repair agent), 12 parts of phenol A type epoxy curing agent, 55 parts of reinforcing material glass fiber, 1 part of leveling agent, and 0.5 parts of defoaming agent;
[0090] The polyester is dissolved in a solvent to form an emulsion, an epoxy resin repair agent is added, and microcapsules are formed by interfacial polymerization or in-situ polymerization. The polyurethane matrix and the curing agent are mixed evenly, and microcapsules, glass fibers, leveling agents and defoaming agents are added, mixed evenly, and allowed to stand at 60°C for 24 hours for curing.
[0091] Sealing ring compound:
[0092] Clean the surface of the rubber ring, use a sprayer to evenly coat the microcapsule composite colloid on the surface of the rubber ring, control the thickness of each layer of colloid to not exceed 0.5mm, ensure that there is no missing area, check and repair after each layer is cured, the total thickness is 3mm, after the composite is completed, grind or polish the surface to make it smooth and flat.
[0093] Equipment installation:
[0094] Install the sealing ring 5 in the outer wall groove 12 of the limiting liquid column 6, place the limiting blocks 4 at both ends of the sealing ring 5, insert the limiting liquid column 6 into the installation groove a10 and the installation groove b11, and use a welding machine to weld the joint 1 and the cylinder body 3.
[0095] Test example:
[0096] The test is to determine whether the sealing ring 5 can restore its sealing performance through a self-repair mechanism after experiencing hydraulic shock.
[0097] The test method comprises the steps of:
[0098] The sealing ring 5 prepared in Example 1 was initially inspected and its surface condition was good. The sealing ring 5 was installed in the groove 12 of the limit liquid column 6 and installed between the joint 1 and the cylinder body 3 to simulate hydraulic shock. The sealing system was connected using a hydraulic test bench to gradually increase the pressure in the system to simulate the normal working pressure (20 MPa). The system pressure was quickly increased to a peak value (50 MPa) to simulate hydraulic shock. The surface changes of the sealing ring (5) before and after the hydraulic shock were recorded.
[0099] Damage condition: After the hydraulic shock, several cracks with a length of about 5 mm appeared on the surface of the sealing ring 5.
[0100] Self-repairing effect: After 48 hours of natural repair, the microcapsules at the cracks rupture and release the repair agent, effectively filling the cracks. The surface of the sealing ring returns to its original smoothness without obvious cracks or openings.
[0101] Sealing test: Under the 30MPa pressure test, the repaired sealing ring 5 did not leak.
[0102] Through the above tests, the durability and self-repairing ability of the sealing ring 5 in actual use can be comprehensively evaluated to ensure that it can still maintain good sealing performance in a complex working environment.
[0103] Sealing test: Under the 30MPa pressure test, the repaired sealing ring 5 did not leak.
[0104] Strength test: The test method is tensile test, and the test result is: breaking strength ≥ 20MPa.
[0105] Durability test: Cyclic pressure test 10,000 times, test results show no obvious wear or leakage.
[0106] Example 2
[0107] Rubber ring preparation:
[0108] The raw materials include 100 parts of fluororubber (FKM), 2.5 parts of sulfur (S), 2 parts of accelerator (CBS), 3 parts of activator (zinc stearate), 1 part of anti-scorch agent (NS), 60 parts of carbon black (N550), 12 parts of paraffin oil, and 1.5 parts of antioxidant RD;
[0109] Put the fluororubber into an internal mixer for plasticization, and gradually add sulfur, accelerator, activator, anti-scorch agent, carbon black, paraffin oil, and antioxidant RD to ensure that each component is evenly dispersed in the rubber matrix. Put the mixed rubber into the vulcanization equipment and vulcanize it at 180℃ and 10MPa pressure for 30 minutes. After the vulcanization is completed, cool the rubber ring to room temperature and check its size and appearance.
[0110] Preparation of microcapsule composite colloid:
[0111] The raw materials include 100 parts of polyurethane (PU), 20 parts of microcapsules (containing epoxy resin repair agent), 15 parts of phenol A type epoxy curing agent, 60 parts of glass fiber, 2 parts of leveling agent, and 1 part of defoaming agent;
[0112] The polyester is dissolved in a solvent to form an emulsion, an epoxy resin repair agent is added, and microcapsules are formed by interfacial polymerization or in-situ polymerization. The polyurethane matrix and the curing agent are mixed evenly, and microcapsules, glass fibers, leveling agents and defoaming agents are added, mixed evenly, and allowed to stand at 60°C for 24 hours for curing.
[0113] Sealing ring compound:
[0114] Clean the surface of the rubber ring, use a sprayer to evenly coat the microcapsule composite colloid on the surface of the rubber ring, control the thickness of each layer of colloid to not exceed 0.5mm, ensure that there is no missing area, check and repair after each layer is cured, the total thickness is 3.5mm, after the composite is completed, grind or polish the surface to make it smooth and flat.
[0115] Equipment installation:
[0116] Install the sealing ring 5 in the outer wall groove 12 of the limiting liquid column 6, place the limiting blocks 4 at both ends of the sealing ring 5, insert the limiting liquid column 6 into the installation groove a10 and the installation groove b11, and use a welding machine to weld the joint 1 and the cylinder body 3.
[0117] Test example:
[0118] The sealing ring 5 prepared in Example 2 was initially inspected and its surface condition was good.
[0119] Install the sealing ring 5 into the groove 12 of the limiting liquid column 6, and install it between the joint 1 and the cylinder body 3 to simulate hydraulic shock. Use a hydraulic test bench to connect the sealing system, gradually increase the pressure in the system to simulate the normal working pressure (20MPa), quickly increase the system pressure to the peak value (50MPa), simulate hydraulic shock, and record the surface changes of the sealing ring 5 before and after the hydraulic shock.
[0120] Damage:
[0121] After the hydraulic shock, several cracks with a length of about 6 mm appeared on the surface of the sealing ring 5.
[0122] Self-repair effect:
[0123] After 48 hours of natural repair, the microcapsules at the cracks ruptured and released the repair agent, effectively filling the cracks. The surface of the sealing ring returned to its original smoothness without obvious cracks or openings.
[0124] Sealing test: Under the 30MPa pressure test, the repaired sealing ring 5 did not leak.
[0125] Strength test: The test method is tensile test, and the test result is: breaking strength ≥ 22MPa.
[0126] Durability test: Cyclic pressure test 10,000 times, test results show no obvious wear or leakage.
[0127] Through the test of Example 2, it can be seen that under different formulations and process parameters, the sealing ring 5 can also show good sealing performance and self-repairing ability. After the hydraulic shock, the sealing ring 5 can restore its surface integrity through the self-repairing mechanism to ensure the sealing effect under high pressure environment. This shows that the present application has wide adaptability and reliability in practical applications.
[0128] Example 3
[0129] Rubber ring preparation
[0130] Raw materials:
[0131] Fluororubber (FKM): 100 parts
[0132] Sulfur (S): 2 parts
[0133] Accelerator (CBS): 2 parts
[0134] Activator (zinc stearate): 2.5 parts
[0135] Anti-scorch agent (NS): 0.75 parts
[0136] Carbon black (N550): 52 parts
[0137] Paraffin oil: 13 parts
[0138] Anti-aging agent RD: 1.2 parts
[0139] Put the fluororubber into the internal mixer for plasticization, gradually add sulfur, accelerator, activator, anti-scorch agent, carbon black, paraffin oil, and antioxidant RD to ensure that each component is evenly dispersed in the rubber matrix, put the mixed rubber into the vulcanization equipment, and vulcanize it at 180℃ and 10MPa pressure for 30 minutes. After the vulcanization is completed, cool the rubber ring to room temperature and check the size and appearance. Preparation of microcapsule composite colloid
[0140] Raw materials:
[0141] Base material: Polyurethane (PU): 100 parts
[0142] Microcapsules (containing epoxy resin repair agent): 18 parts
[0143] Phenol A type epoxy curing agent: 14 parts
[0144] Reinforcement material: Glass fiber: 58 parts
[0145] Leveling agent: 1.5 parts
[0146] Defoamer: 0.75 parts
[0147] Preparation process:
[0148] The polyester is dissolved in a solvent to form an emulsion, an epoxy resin repair agent is added, and microcapsules are formed by interfacial polymerization or in-situ polymerization. The polyurethane matrix and the curing agent are mixed evenly, and the microcapsules, glass fibers, leveling agents and defoaming agents are added and mixed evenly.
[0149] Allow to cure at 60°C for 24 hours.
[0150] Sealing ring compound
[0151] Coating steps:
[0152] Clean the surface of the rubber ring, use a sprayer to evenly coat the microcapsule composite colloid on the surface of the rubber ring, control the thickness of each layer of colloid to not exceed 0.5mm, ensure that there is no missing area, check and repair after each layer is cured, the total thickness is 3.2mm, after the composite is completed, grind or polish the surface to make it smooth and flat.
[0153] Equipment Installation
[0154] Installation steps:
[0155] Install the sealing ring 5 in the outer wall groove 12 of the limiting liquid column 6, place the limiting blocks 4 at both ends of the sealing ring 5, insert the limiting liquid column 6 into the installation groove a10 and the installation groove b11, and use a welding machine to weld the joint 1 and the cylinder body 3.
[0156] Test example:
[0157] The sealing ring 5 prepared in Example 2 was initially inspected and its surface condition was good.
[0158] Install the sealing ring 5 into the groove 12 of the limiting liquid column 6, and install it between the joint 1 and the cylinder body 3, simulate hydraulic shock, use a hydraulic test bench to connect the sealing system, gradually increase the pressure in the system, and simulate the normal working pressure (20MPa).
[0159] Rapidly increase the system pressure to a peak value (50 MPa) to simulate hydraulic shock, and record the surface changes of the sealing ring 5 before and after the hydraulic shock.
[0160] Damage:
[0161] After the hydraulic shock, several cracks with a length of about 5 mm to 6 mm appeared on the surface of the sealing ring 5.
[0162] Self-repair effect:
[0163] After 48 hours of natural repair, the microcapsules at the cracks ruptured and released the repair agent, effectively filling the cracks. The surface of the sealing ring returned to its original smoothness without obvious cracks or openings.
[0164] Sealing test:
[0165] Under the 30 MPa pressure test, the repaired sealing ring 5 did not leak.
[0166] Strength test: The test method is tensile test, and the test result is: breaking strength ≥ 21MPa.
[0167] Durability test: Cyclic pressure test 10,000 times, test results show no obvious wear or leakage.
[0168] Through the test of Example 3, it can be seen that under different formulations and process parameters, the sealing ring 5 can also show good sealing performance and self-repairing ability. After the hydraulic shock, the sealing ring 5 can restore its surface integrity through the self-repairing mechanism to ensure the sealing effect under high pressure environment. This shows that the present application has wide adaptability and reliability in practical applications. Through the comparison of different embodiments, it can be found that even under different formulations and process conditions, the sealing ring can still meet high-standard performance requirements.
Claims
1. A new type of column jack joint welding system, It is characterized in that The invention comprises a cylinder body (3), wherein a joint (1) is fixedly provided on the outer wall of the cylinder body (3), a joint liquid passage hole (2) is provided inside the joint (1), a cylinder liquid passage hole (3-1) is provided on the cylinder body (3), the joint liquid passage hole (2) and the cylinder liquid passage hole (3-1) are connected via a limiting liquid passage column (6), a limiting column liquid passage hole (7) is provided inside the limiting liquid passage column (6), and the limiting column liquid passage hole (7) is connected to the joint liquid passage hole (2) and the cylinder liquid passage hole (3-1).
2. A novel column jack joint welding system according to claim 1, It is characterized in that The outer wall of the limiting liquid column (6) is provided with a plurality of annular grooves (12), a matching sealing ring (5) is installed in the groove (12), and limiting blocks (4) are provided at both ends of the sealing ring (5).
3. A novel column jack joint welding system according to claim 1, It is characterized in that The joint liquid passage hole (2) is L-shaped.
4. A novel column jack joint welding system according to claim 1, It is characterized in that The end of the joint liquid-passing hole (2) close to the cylinder body (3) is provided with a mounting groove a (10), the end of the cylinder body liquid-passing hole (3-1) close to the joint (1) is provided with a mounting groove b (11) corresponding to the mounting groove a (10), and the two ends of the position-limiting liquid-passing column (6) are correspondingly mounted in the mounting groove a (10) and the mounting groove b (11).
5. A novel column jack joint welding system according to claim 4, It is characterized in that The outer contour of the position-limiting liquid column (6) is a non-cylindrical column, the installation groove a (10) and the installation groove b (11) for installing the position-limiting liquid column (6) are installation grooves that match the outer contour of the position-limiting liquid column (6), and the position-limiting column liquid hole (7) is a circular hole that is compatible with the joint liquid hole (2) and the cylinder body liquid hole (3-1).
6. A novel column jack joint welding system according to claim 5, It is characterized in that The outer contour of the limit liquid column (6) is an elliptical cylinder, and the mounting groove b (11) on the outer side of the cylinder body liquid hole (3-1) and the mounting groove a (10) at the lower end of the joint liquid hole (2) are corresponding elliptical mounting grooves.
7. A novel column jack joint welding system according to claim 2, It is characterized in that The sealing ring (5) comprises an inner ring and an outer ring, wherein the inner ring is made of rubber and the outer ring is made of a microcapsule composite material. The inner ring and the outer ring are combined by coating the microcapsule composite colloid on the outer surface of the rubber ring, coating the second layer of the microcapsule composite colloid after the first layer of the microcapsule composite colloid is solidified, coating the third layer of the microcapsule composite colloid after the second layer of the microcapsule composite colloid is solidified, and the cycle is repeated until the size requirement is met.
8. A novel column jack joint welding system according to claim 7, It is characterized in that The preparation method of the rubber ring includes: firstly plasticizing the fluororubber, then gradually adding sulfur, accelerator, activator, anti-scorch agent, carbon black, paraffin oil, and antioxidant RD, uniformly dispersing the components in the rubber matrix for mixing, then putting the mixed rubber into the vulcanization equipment for vulcanization treatment, and after the vulcanization is completed, cooling the rubber ring to room temperature to obtain the rubber ring.
9. A novel column jack joint welding system according to claim 8, It is characterized in that The weight ratio of each component of the rubber ring is: Fluororubber: 100 parts; Sulfur: 1-2 parts; Accelerator: 1.5-2 parts; Activator: 2-5 parts; Anti-scorching agent: 0.5-1 part; Carbon black: 50-55 parts; Paraffin oil: 10-15 parts; Anti-aging agent RD: 1-2 parts.
10. A novel column jack joint welding system according to claim 7, It is characterized in that The preparation method of the microcapsule composite colloid comprises: dissolving polyester in a solvent to form an emulsion, adding an epoxy resin repair agent into the emulsion, and then forming microcapsules of the polyester around the epoxy resin repair agent through interfacial polymerization or in-situ polymerization; mixing a polyurethane matrix and a curing agent evenly, and then adding microcapsules, glass fibers, a leveling agent and a defoaming agent, and continuing to stir until evenly dispersed to obtain a microcapsule composite colloid.