Additive manufacturing method for dissimilar steel semi-guide vane of water pump turbine seat ring

Through the additive manufacturing method of different steel semiconductor vanes, the problems of poor manufacturing processability and low operating safety margin of traditional water pump turbine seat ring are solved, and the different metal structure design of carbon steel ring plate and stainless steel vanes are realized, which improves welding efficiency and machinery Performance, improves manufacturing quality and safety margin.

CN119057408APending Publication Date: 2024-12-03CHINA THREE GORGES PROJECTS DEV CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411463315.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The manufacturing process of traditional water pump turbine seat rings is poor, the welding and grinding difficulty is high, the operation safety margin is low, and the different metal structure functional design of carbon steel ring plates and stainless steel guide vanes with stronger corrosion resistance is not possible.

Method used

Adopting the additive manufacturing method of different steel semiconductor blades, the transition layer of austenite welding material is surfacing the groove at the outer contour milling of the root of the guide blade, and the multi-robot synchronously welded the martensitic stainless steel semiconductor blades by layer-by-layer additive welding. , followed by stress-removing heat treatment and laser-arc composite welding to form a different metal structure of carbon steel ring plate and stainless steel guide vane.

Benefits of technology

It reduces the welding and grinding workload, improves manufacturing quality and operation safety margin, realizes automated welding, shortens process cycle, and improves mechanical performance and non-destructive testing purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057408A_ABST
    Figure CN119057408A_ABST
Patent Text Reader

Abstract

The invention discloses a pump turbine seat ring dissimilar steel semi-guide vane additive manufacturing method. Compared with a steel plate welding structure seat ring, an automatic welding method is easy to realize, and the manufacturability of welding, grinding, nondestructive testing and other procedures of the ring plate and the guide vane is also improved; compared with a seat ring of a split casting welding structure or a seat ring of an integral casting structure, the seat ring has the advantages that the mechanical property, the tissue density and the nondestructive testing purity of a guide vane base material are improved, the dissimilar metal structure function design and the manufacturing process of the carbon steel ring plate and the stainless steel guide vane with higher corrosion resistance are realized, and the corrosion resistance and the cavitation resistance of the guide vane are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of water pump turbines, and in particular to a method for additively manufacturing heterogeneous steel semi-guide vanes of a water pump turbine seat ring. Background Art

[0002] The high stress area of ​​the pump turbine seat ring welding and operation is located in the transition arc area at the root of the guide vane. The stress amplitude decreases from the transition arc to the ring plate and the two sides of the guide vane. The stress ratio △σ / △σmax at the center line of the seat ring water guide mechanism is less than 0.5. The pump turbine seat ring is generally a steel plate welding structure, a split casting welding structure or a whole casting structure. The steel plate welding structure seat ring includes an upper ring plate 1, a lower ring plate 2 and a guide vane 3. The connecting weld 4 between the guide vane and the ring plate is in the form of a T-joint; the split casting welding structure seat ring includes a seat ring upper half 5 and a seat ring lower half 6. The connecting weld 7 between the two is located at the center line of the seat ring water guide structure. Its disadvantages are:

[0003] 1) The connecting weld is located in the transition arc area at the root of the guide vane. The high stress area of ​​the seat ring welding and operation is highly overlapped with the T-type connecting weld between the ring plate and the guide vane. The high stress acts on the weak structure inside the T-type connecting weld, posing a risk to the safe and stable operation of the unit.

[0004] 2) For the pump turbine seat ring with small guide vane opening D, chord distance S, and long flow channel L, the manufacturing process of welding, grinding and non-destructive testing of the ring plate and guide vane is poor.

[0005] 3) The mechanical properties of the ring plate and guide vane parent materials made of castings are poor, generally lower than the connecting welds between the ring plate and the guide vanes. At the same time, the tissue density and non-destructive testing purity of the ring plate and guide vane parent materials made of castings are poor, and there are relatively more original casting defects.

[0006] 4) There are many welding seams between the ring plate and the guide vane, the amount of deposited metal at the joint is large, the welding and transition arc grinding cycle is long, and the line size and surface finish of the manually polished transition arc are difficult to guarantee.

[0007] 5) It is difficult to apply automated welding methods to the T-type connection weld between the guide vane and the ring plate. The quality of manual welding is difficult to guarantee and the welding efficiency is low.

[0008] 6) The pump turbine seat ring with a split casting welding structure or an integral casting structure cannot realize the functional design and manufacturing process of the dissimilar metal structure of the carbon steel ring plate and the stainless steel guide vane with stronger corrosion resistance.

[0009] In summary, the manufacturing process of the pump-turbine seat ring using the traditional welding structure and manufacturing method is poor, the welding and grinding are difficult and the cycle is long, and the safety margin of component manufacturing and operation is relatively low. Therefore, it is necessary to develop a new method for manufacturing the pump-turbine seat ring. Summary of the invention

[0010] In view of this, the present invention adopts a new method for manufacturing a seat ring of a water pump turbine, which can replace the seat ring of a water pump turbine with a traditional welding structure and manufacturing method, improves the manufacturing processability of the seat ring product, and realizes the dissimilar metal structure function design and manufacturing process of the seat ring carbon steel ring plate and the stainless steel guide vane while reducing the workload and difficulty of welding and grinding, realizes the automatic welding of the guide vane additive and the butt welds between the guide vanes, and improves the manufacturing quality of the seat ring product and the safety margin of operation. The technical solution of the present invention is: the upper ring plate, the lower ring plate and the guide vane are divided into an upper half and a lower half with the center line of the seat ring water guide mechanism as the boundary, the upper half and the lower half are independently manufactured and a half guide vane is integrally arranged, the half guide vane body and the transition arc at the root are prepared by additive, and the upper half and the lower half are welded into a whole by welding the connecting weld at the center line of the seat ring water guide mechanism.

[0011] Step 1: The guide vane and the ring plate are assembled by milling a groove according to the outer contour of the transition arc at the root of the guide vane;

[0012] Step 2: Using austenitic welding materials to build up a transition layer at the grooves of the upper half ring plate and the lower half ring plate;

[0013] Step 3: The upper and lower half guide vanes made of martensitic stainless steel are welded layer by layer by multiple robots in a back-to-back state;

[0014] Step 4: After the half guide vane is welded, it is subjected to stress relief heat treatment, and then the upper and lower halves are separated, and then the guide vane contour surface and the connecting weld groove are processed;

[0015] Step 5: Finally, multiple robots are used to simultaneously weld the connecting weld between the upper and lower halves using a laser and arc hybrid welding method.

[0016] In the above-mentioned additive manufacturing method for heterogeneous steel semi-guide vanes of a pump turbine seat ring, the inclination angle of the side wall of the transition layer surfacing groove in step one is not less than 45 degrees, and the depth is not less than 5 mm.

[0017] In the above-mentioned method for additive manufacturing of heterogeneous steel semi-guide vanes of a water pump turbine seat ring, in the step 2, the ferrite content of the transition layer surfacing austenitic welding material is above 10%.

[0018] In the above-mentioned method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump-turbine seat ring, the back-to-back state of the upper half and the lower half in step three is that the upper plane of the upper half ring plate is in contact with the lower plane of the lower half ring plate and is lap-welded into a whole.

[0019] In the above-mentioned method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump-turbine seat ring, the semi-guide vane additive welding method in step three is a laser composite arc, and the additive welding path is planned to be perpendicular to the normal direction of the guide vane thickness.

[0020] In the above-mentioned additive manufacturing method of the heterogeneous steel semi-guide vanes of the water pump turbine seat ring, the connecting weld joint form and welding position between the upper half and the lower half in step five are narrow gap butt transverse weld joints.

[0021] The beneficial effects of the present invention compared with the prior art are:

[0022] 1. The present invention proposes an additive manufacturing method for a water pump turbine seat ring of heterogeneous steel semi-guide vanes. Compared with a seat ring with a steel plate welded structure, the seat ring connecting weld avoids the high stress area of ​​the seat ring operation, thereby improving the manufacturing quality of the seat ring product and the safety margin of operation.

[0023] 2. The present invention proposes an additive manufacturing method for a half-guide vane of a water pump turbine seat ring made of heterogeneous steel. Compared with a seat ring with a steel plate welded structure, the T-shaped connecting weld 4 between the ring plate and the guide vane is transformed into a butt joint between the upper and lower guide vanes, thereby reducing the difficulty of welding and grinding the transition arc at the root of the guide vane, making it easy to realize an automated welding method, and also improving the manufacturing processability of the processes of welding, grinding and non-destructive testing of the ring plate and the guide vane.

[0024] 3. The present invention proposes an additive manufacturing method for the heterogeneous steel semi-guide vanes of a water pump turbine seat ring. Compared with the seat ring of a steel plate welded structure, the number of connecting welds is reduced by half, the welding and grinding cycle is shortened, and at the same time, the transition arc profile size and surface finish of the guide vane root are changed from manual grinding to mechanical processing, with higher precision.

[0025] 4. The present invention proposes a method for additive manufacturing of heterogeneous steel semi-guide vanes for a pump turbine seat ring. Compared with seat rings with split casting welding structures or integral casting structures, the guide vane base material prepared by laser composite arc additive welding has better mechanical properties, organizational density, and purity during non-destructive testing.

[0026] 5. The present invention proposes an additive manufacturing method for a water pump turbine seat ring made of heterogeneous steel semi-guide vanes. Compared with a seat ring with a split casting welding structure or a whole casting structure, the laser composite arc additive welding method can realize a heterogeneous metal structural functional design and manufacturing process of a carbon steel ring plate and a stainless steel guide vane with stronger corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the steel plate welded structure seat ring.

[0028] Figure 2 It is a schematic diagram of a seat ring of a split casting welding structure or an integral casting structure.

[0029] Figure 3 Schematic diagram of ring plate milling and transition layer surfacing.

[0030] Figure 4 Schematic diagram of guide vane additive manufacturing.

[0031] Figure 5 This is a schematic diagram of the welding of the upper and lower halves.

[0032] Description of components in the figure: 1-upper ring plate; 2-lower ring plate; 3-guide vane; 4-connecting weld between guide vane and ring plate; 5-upper half of seat ring of split casting welding structure; 6-lower half of seat ring of split casting welding structure; 7-connecting weld between upper and lower halves of seat ring of split casting welding structure; 8-upper half; 9-lower half; 10-half guide vane; 11-transition arc at the root of guide vane; 12-connecting weld between upper and lower halves; 13-guide vane; 14-ring plate; 15-outer contour of transition arc at the root of guide vane; 16-groove; 17-upper half ring plate; 18-lower half ring plate; 19-transition layer; 20-guide vane contour surface. DETAILED DESCRIPTION

[0033] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0034] Specific implementation method 1: Figure 1 , Figure 3 , Figure 5 , the upper ring plate 1, the lower ring plate 2 and the guide vane 3 are divided into two parts, the upper half 8 and the lower half 9, with the center line of the seat ring water guide mechanism as the boundary. The upper half 8 and the lower half 9 are independently manufactured and integrally provided with a semi-guide vane 10. The semi-guide vane 10 body and the root transition arc 11 are prepared by additive manufacturing. The upper half 8 and the lower half 9 are welded into a whole by welding the connecting weld 12 at the center line of the seat ring water guide mechanism. The effect of this embodiment is to reduce the number of seat ring connecting welds 12 by half, shortening the welding and grinding cycle; at the same time, the seat ring connecting weld 12 avoids the high stress area of ​​the seat ring operation, and the stress amplitude at the position of the connecting weld 12 is lower than 1 / 2 of the highest stress value at the position of the transition arc 11 at the root of the guide vane, thereby improving the manufacturing quality of the seat ring product and the safety margin of operation.

[0035] The method for additive manufacturing of a water pump turbine seat ring heterogeneous steel semi-guide vane provided in this embodiment is achieved by the following steps:

[0036] Step 1: If Figure 3 and Figure 4 As shown, the assembly position of the guide vane 13 and the ring plate 14 is milled with a groove 16 according to the transition arc outer contour 15 of the guide vane root.

[0037] Step 2: If Figure 3 As shown, austenitic welding materials are used to build up the transition layer 19 at the grooves 16 of the upper semi-ring plate 17 and the lower semi-ring plate 18; the purpose of using austenitic welding materials to build up the transition layer 19 at the grooves in this step is to ensure the additive welding quality of the semi-guide vane 10 made of martensitic stainless steel.

[0038] Step 3: If Figure 5 As shown, the upper half 8 and the lower half 9 are synchronously additively welded layer by layer by multiple robots in a back-to-back state. The purpose of using multiple robots in this step is to improve the efficiency of additive manufacturing. The purpose of using additive welding to prepare the martensitic stainless steel semi-guide vane 10 is to achieve a more corrosion-resistant carbon steel ring plate and a stainless steel guide vane with a dissimilar metal structure function design and manufacturing process, and to improve the guide vane's resistance to wear and cavitation.

[0039] Step 4: If Figure 5 As shown, the semi-guide vane 10 is subjected to stress relief heat treatment after additive welding, and then the upper half 8 and the lower half 9 are disassembled and separated, and then the guide vane contour surface 20 and the groove of the connecting weld 12 are processed; in this step, the role of the stress relief heat treatment after the semi-guide vane 10 is to eliminate welding residual stress and stabilize the processing size of the guide vane contour surface 20 and the groove of the connecting weld 12; the role of the mechanical processing of the semi-guide vane 10 additive welding surface is to improve the profile size and surface finish of the transition arc 11 at the root of the guide vane.

[0040] Step 5: If Figure 5 As shown, finally, a laser and arc composite welding method is adopted to synchronously weld the connecting weld 12 between the upper half 8 and the lower half 9 by multiple robots; the purpose of using a laser and arc composite welding method to synchronously weld the connecting weld 12 between the upper half 8 and the lower half 9 by multiple robots in this step is to improve the mechanical properties of the connecting weld 12 between the upper half 8 and the lower half 9 by adopting a special welding method.

[0041] Specific implementation method 2: Figure 3 As shown, this embodiment further limits step one described in specific embodiment one. In this embodiment, the transition layer 19 in step one has a side wall inclination angle α of not less than 45 degrees, and a depth H1 of not less than 5 mm. The transition layer 19 in this step has a side wall inclination angle α of not less than 45 degrees, and a depth H1 of not less than 5 mm, which is to improve the operational processability of the surfacing of the austenite transition layer 19 at the groove 16.

[0042] Specific implementation method three: Figure 3 As shown, this embodiment further limits step two described in specific embodiment one. In this embodiment, in step two, the ferrite content of the austenitic welding material for surfacing the transition layer 19 is above 10%. In this step, the ferrite content of the austenitic welding material for surfacing the transition layer 19 is above 10% to avoid welding thermal cracks caused by surfacing the transition layer 19 and ensure the surfacing quality of the transition layer 19.

[0043] Specific implementation method four: Figure 5As shown, this embodiment further limits step two described in specific embodiment one. In this embodiment, the back-to-back state of the upper half 8 and the lower half 9 in step three is that the upper plane of the upper half ring plate 17 is in contact with the lower plane of the lower half ring plate 18 and is overlap-welded into a whole; the purpose of the back-to-back state of the upper half 8 and the lower half 9 in this step is to reduce the deformation of additive welding.

[0044] Specific implementation method five: Figure 3 and Figure 4 As shown, this embodiment further limits step 2 described in specific embodiment 1. In this embodiment, the additive welding method for the semi-guide vane 10 in step 3 is laser composite arc, and the additive welding path is planned to be perpendicular to the thickness normal of the guide vane 13; in this step, the semi-guide vane 10 adopts the laser composite arc additive welding method to improve the mechanical properties of the guide vane base material, the density of the organization, and the purity of non-destructive testing; the additive welding path is planned to be perpendicular to the thickness normal of the guide vane 13 to prevent the flow of cladding metal at the edge position, improve the deposition effect of the cladding weld, and thereby improve the forming quality of the welding surface.

[0045] Specific implementation method six: Figure 5 As shown, this embodiment further limits step two described in specific embodiment one. In this embodiment, in step five, the joint form and welding position of the connecting weld 12 between the upper half 8 and the lower half 9 are narrow gap butt transverse welding joints; in this step, the joint form and welding position of the connecting weld 12 between the upper half 8 and the lower half 9 are narrow gap butt transverse welding joints, which reduces the difficulty of welding and grinding the transition arc at the root of the guide vane, makes it easy to implement an automated welding method, and also improves the manufacturing processability of the processes such as welding, grinding and non-destructive testing of the ring plate and the guide vane.

[0046] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0047] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0048] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump turbine seat ring, characterized in that: The upper ring plate (1), the lower ring plate (2) and the guide vane (3) are divided into an upper half (8) and a lower half (9) with the center line of the seat ring water guide mechanism as the boundary. The upper half (8) and the lower half (9) are independently manufactured and integrally provided with a half guide vane (10). The body of the half guide vane (10) and the transition arc (11) at the root are prepared by additive manufacturing. The upper half (8) and the lower half (9) are welded into a whole by welding a connecting weld (12) at the center line of the seat ring water guide mechanism. The method is implemented by the following steps: Step 1: The guide vane (13) and the ring plate (14) are assembled by milling a groove (16) according to the outer contour of the transition arc at the root of the guide vane (15); Step 2: Using austenitic welding materials to build up a transition layer (19) at the grooves (16) of the upper half ring plate (17) and the lower half ring plate (18); Step 3: The upper half (8) and the lower half (9) are back-to-back welded by multiple robots layer by layer to form a half guide vane (10) made of martensitic stainless steel; Step 4: After the half guide vane (10) is additively welded, it is subjected to stress relief heat treatment, and then the upper half (8) and the lower half (9) are separated, and then the guide vane contour surface (20) and the groove of the connecting weld (12) are processed; Step 5: Using a laser and arc composite welding method, multiple robots synchronously weld the connecting weld (12) between the upper half (8) and the lower half (9).

2. The method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump turbine seat ring according to claim 1, characterized in that: In the step 1, the inclination angle α of the side wall of the transition layer (19) surfacing groove (16) is not less than 45 degrees, and the depth H1 is not less than 5 mm.

3. The method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump turbine seat ring according to claim 1, characterized in that: In the step 2, the ferrite content of the transition layer (19) surfacing austenitic welding material is above 10%.

4. The method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump turbine seat ring according to claim 1, characterized in that: In the step three, the upper half (8) and the lower half (9) are in a back-to-back state, with the upper plane of the upper half ring plate (17) and the lower plane of the lower half ring plate (18) in contact and overlap-welded into a whole.

5. The method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump turbine seat ring according to claim 1, characterized in that: In the step three, the additive welding method of the semi-guide vane (10) is a laser composite arc, and the additive welding path is planned to be perpendicular to the thickness normal of the guide vane (13).

6. The method for additive manufacturing of heterogeneous steel semi-guide vanes of a pump turbine seat ring according to claim 1, characterized in that: In the step 5, the joint form and welding position of the connecting weld (12) between the upper half (8) and the lower half (9) are narrow gap butt transverse weld joints.

Citation Information

Patent Citations

  • Blading with branches on the shroud of an axial-flow turbomachine compressor

    CN105275501A

  • Guide baffle of turbo-machine and method for producing same

    CN110529193A

  • Water pump turbine seat ring of cast-weld structure and manufacturing method of water pump seat ring

    CN115163563A

  • Electric arc material increasing method of martensitic stainless steel impeller blade

    CN117324724A