High-smoothness tempered glass and preparation method thereof

By adopting three-layer structure composite glass, using the high softening point temperature of the intermediate layer glass as support, combined with multi-layer kiln and tempering furnace technology, the problem of warping and deformation of thin glass during tempering is solved, and high strength and high strength are achieved Flat tempered glass, suitable for lightweight photovoltaic modules.

CN119058187APending Publication Date: 2024-12-03CHANGZHOU ALMADEN
View PDF 0 Cites -1 Cited by

Patent Information

Application Number
CN202411242213.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Thin glass is prone to warping and deformation of the edges during tempering, resulting in low flatness and difficult to meet the development needs of lightweight photovoltaic modules.

Method used

The composite glass with a three-layer structure is adopted. The softening point temperature of the intermediate glass is higher than that of the upper and lower surface glass. It forms compressive stress through uniform cooling. Combined with the technology of multi-layer kilns and tempering furnaces, the high strength and flatness of the glass are ensured.

Benefits of technology

High-level tempered glass with high strength, low fracture possibility and excellent thermal insulation effect has durability comparable to thicker and heavier glass, and significantly improves the flatness of the tempered glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119058187A_ABST
    Figure CN119058187A_ABST
Patent Text Reader

Abstract

The invention discloses high-flatness tempered glass and a preparation method thereof. The tempered glass is of an integrated composite glass structure formed by tempering and forming n layers of laminated glass, the softening point temperature of the middle-layer glass is higher than that of the upper and lower surface-layer glass, and the tempering forming temperature is within the softening point temperature interval of the surface-layer glass; n > = 3. The preparation method comprises the following steps: S1, respectively proportioning the raw material components of the upper surface layer glass, the middle layer glass and the lower surface layer glass, and stirring and mixing; s2, feeding the mixed raw materials into a multi-layer kiln for melting to form three kinds of uniform bubble-free molten glass; s3, feeding the molten glass into a distributor at the inlet of the forming pool, distributing the molten glass obtained after the upper surface layer glass is molten to the upper layer, distributing the molten glass obtained after the middle layer glass is molten to the middle layer, distributing the molten glass obtained after the lower surface layer glass is molten to the lower layer, conveying the molten glass to the same lip for convergence, performing multi-layer shaping, and then cooling and forming; and S4, carrying out cooling molding, and then carrying out tempering so as to prepare the high-flatness tempered glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tempered glass, and in particular to a tempered glass with high flatness and a preparation method thereof. Background Art

[0002] At present, photovoltaic modules are gradually developing towards the trend of lightweighting. By reducing the dead weight of the modules, the load of the modules on the bracket system is reduced to adapt to more scenarios and application environments. However, in order to reduce the weight of the modules and avoid damage, photovoltaic module manufacturers usually add aluminum frames to double-glass photovoltaic modules, and reduce the thickness of the glass used in the modules to 2.0mm or even thinner. During the tempering process of thin glass, the tempering furnace heats to a softened state and then enters a cooling state. Due to the different cooling rates or temperatures of the upper and lower surfaces, one side solidifies first and the other side continues to shrink. This can easily cause the tempered glass to deform upward or downward, thus forming a concave surface, that is, the edge warping and deformation, and low flatness. Summary of the invention

[0003] The purpose of the present invention is to propose a highly flat tempered glass and a preparation method thereof to address the problem that the existing thin glass is prone to edge warping and deformation during the tempering process, resulting in low flatness, so as to make it suitable for the development trend of lightweight photovoltaic modules.

[0004] To achieve the above object, the present invention is implemented by the following technical solutions:

[0005] The present invention provides a highly flat tempered glass, which is an integrated composite glass structure formed by tempering and molding n layers of laminated glass;

[0006] Among them, the middle layer of glass plays a supporting role in the glass tempering process, the softening point temperature of the middle layer of glass is higher than the softening point temperatures of the upper and lower surface glasses, and the tempering molding temperature is in the softening point temperature range of the surface glasses; wherein n is a positive integer and satisfies n≥3.

[0007] Physical tempering of glass is to heat the glass to the softening temperature, and then quickly and evenly cool the glass surface to shrink it, forming compressive stress on the glass surface. When the heating or force or wind pressure is uneven, waveforms and warping will appear. The thinner the glass, the more difficult it is to ensure the flatness of the glass because the tempering parameters will be adjusted to achieve the glass strength.

[0008] In order to solve the problem of warping and deformation of the edges of the thin glass mentioned above and improve its flatness after tempering, the present invention proposes a highly flat tempered glass, which is a high-strength composite glass with the advantages of light weight, low possibility of breakage, and excellent thermal insulation effect; at the same time, the composite glass also has a durability comparable to thicker and heavier glass.

[0009] Furthermore, a highly flat tempered glass: the thickness of the middle layer of glass accounts for 40.0-70.0% of the total thickness of the highly flat tempered glass.

[0010] Furthermore, a highly flat tempered glass is provided: the highly flat tempered glass is a composite glass with a three-layer structure, comprising an upper surface glass, an intermediate layer glass and a lower surface glass stacked in sequence; the softening point temperature of the intermediate layer glass is higher than the softening point temperatures of the upper surface glass and the lower surface glass.

[0011] Furthermore, a highly flat tempered glass: the components of the upper surface glass and the lower surface glass are consistent, and they respectively include the following components: SiO2: 70.0~82.0wt%; Al2O3: 0.1~5.0wt%; CaO: 5.0~10.0wt%; MgO: 1.0~5.0wt%; Ni2O3: 0.1~1.0wt%; K2O: 0~1.0wt%; CeO2: 0~0.2wt%; B2O3: 0~1.0wt%; CuO: 0~0.1wt%; SrO: 0.01~2.0wt% and Na2O: 1.0~5.0wt%.

[0012] Furthermore, a highly flat tempered glass: the intermediate layer glass comprises the following components: SiO2: 55.0-68.0wt%; Al2O3: 10.0-20.0wt%; Na2O: 9.0-16.0wt%; CaO: 5.0-9.0wt%; MgO: 1.0-5.0wt%; K2O: 0-1.0wt%; CeO2: 0-0.2wt%; B2O3: 0-1.0wt%; the components of the intermediate layer glass satisfy (SiO2+Al2O3+Na2O)≥85.0wt%.

[0013] The present invention also provides a method for preparing high-flatness tempered glass, the method comprising the following steps:

[0014] S1. Batching: batching the raw materials of the upper surface glass, the middle layer glass and the lower surface glass respectively, and then conveying them to a mixing and stirring machine respectively for uniform stirring and mixing;

[0015] S2, melting: sending the mixed raw materials into a multi-layer furnace for melting to form three kinds of uniform bubble-free glass liquids respectively;

[0016] S3, cooling and molding: the three kinds of glass liquid are sent to the distributor at the entrance of the molding pool, the glass liquid after the upper surface glass is melted is distributed to the upper layer, the glass liquid after the middle layer glass is melted is distributed to the middle layer, and the glass liquid after the lower surface glass is melted is distributed to the lower layer, and they are transported to the same lip to merge, and multi-layer shaping is performed, and then cooled and molded;

[0017] S4, tempering: the multi-layer composite glass obtained by the above cooling and forming is sent to a tempering furnace for tempering and forming, so as to obtain a highly flat tempered glass; the tempering temperature is close to the softening point temperature of the upper and lower surface glasses, and lower than the softening point temperature of the middle layer glass.

[0018] Furthermore, a method for preparing a highly flat tempered glass: the melting temperature in step S2 is 800-1500°C.

[0019] The preparation method of the present invention comprises the following steps: respectively mixing the glass raw materials of each layer evenly, respectively putting them into a multi-layer kiln, the melting temperature of each layer is 800-1500°C, and each layer of glass liquid enters the same multi-layer forming pool at the same time. The distributor at the entrance of the forming pool distributes the molten glass liquid of the upper surface layer to the upper layer, distributes the molten glass liquid of the middle layer to the middle layer, distributes the molten glass liquid of the lower surface layer to the lower layer, and transports them to the same lip for merging, performs multi-layer shaping, and then cools and shapes, cuts, and grinds the edges to obtain a multi-layer composite glass, and then the composite glass is sent to a tempering furnace for tempering, and the tempering temperature is not higher than the softening point temperature of the middle layer of glass.

[0020] Beneficial effects of the present invention:

[0021] (1) The highly flat tempered glass provided by the present invention is formed by integrally molding an upper surface glass, an intermediate layer glass and a lower surface glass, wherein the softening point temperature of the intermediate layer glass is higher than that of the upper surface glass and the lower surface glass. The present invention designs the intermediate layer glass with a high softening point as a support body during physical tempering, which can improve the flatness of the tempered thin glass.

[0022] (2) The advantage of high-strength tempered inhomogeneous glass is that the low softening point components of the upper and lower surface glass cause the glass surface to shrink sharply after the transition temperature to form compressive stress. At the same time, the middle layer of high softening point glass has a high-strength supporting effect when the low softening point components have not reached the softened state at the transition temperature. During cooling, the middle layer of glass acts as a support to firmly fix the low softening point glass on the surface of the high softening point glass, thereby achieving high flatness of the tempered glass surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 This is a schematic structural diagram of a highly flat tempered glass provided in Example 1 of the present invention, that is, a composite glass with a three-layer structure.

[0025] Markings in the figure: 1-composite glass, 11-upper surface glass, 12-middle layer glass, 13-lower surface glass. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In the description of the present invention, it should be understood that the terms "upper", "lower", "left", "right", "top", "bottom", etc., indicating the position or positional relationship, are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Moreover, the terms "first", "second", etc. are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.

[0028] Example 1

[0029] like Figure 1 As shown, this embodiment 1 provides a highly flat tempered glass, which is an integrated composite glass structure formed by tempering three layers of laminated glass, including an upper surface glass 11, an intermediate layer glass 12 and a lower surface glass 13 laminated in sequence;

[0030] The total thickness of the high-flatness tempered glass is 1.8 mm, and the thickness of the middle layer of glass accounts for about 66.7% of the total thickness, that is, the thickness of the upper surface glass 11 is 0.3 mm, the thickness of the middle layer of glass 12 is 1.2 mm, and the thickness of the lower surface glass 13 is 0.3 mm;

[0031] The intermediate layer of glass 12 plays a supporting role in the glass tempering process. The softening point temperature of the intermediate layer of glass 12 is higher than the softening point temperatures of the upper surface layer of glass 11 and the lower surface layer of glass 13. The tempering molding temperature is near the softening point temperatures of the upper surface layer of glass 11 and the lower surface layer of glass 13.

[0032] The components of the upper surface glass 11 and the lower surface glass 13 are consistent, and they respectively include the following components: SiO2: 75.0wt%; Al2O3: 5.0wt%; CaO: 8.0wt%; MgO: 5.0wt%; Ni2O3: 0.5wt%; K2O: 0.5wt%; CeO2: 0.2wt%; B2O3: 0.5wt%; CuO: 0.1wt%; SrO: 1.2wt% and Na2O: 4.0wt%;

[0033] The intermediate layer glass 12 includes the following components: SiO2: 62.0wt%; Al2O3: 15.0wt%; Na2O: 12.0wt%; CaO: 7.0wt%; MgO: 3.0wt%; K2O: 0.5wt%; CeO2: 0.1wt%; B2O3: 0.4wt%, and the components of the intermediate layer glass 12 satisfy (SiO2+Al2O3+Na2O)≥85.0wt%.

[0034] The method for preparing the highly flat tempered glass in the above-mentioned embodiment 1 comprises the following steps:

[0035] S1. Batching: batching the upper surface glass 11, the middle layer glass 12 and the lower surface glass 13 according to their raw material components, and then conveying them to a mixing and stirring machine respectively for uniform stirring and mixing;

[0036] S2, melting: sending the mixed raw materials into a multi-layer furnace for melting at 1200° C. to form three kinds of uniform bubble-free glass liquids respectively;

[0037] S3, cooling and molding: the three kinds of glass liquid are sent to the distributor at the entrance of the molding pool, the glass liquid after the upper surface glass is melted is distributed to the upper layer, the glass liquid after the middle layer glass is melted is distributed to the middle layer, and the glass liquid after the lower surface glass is melted is distributed to the lower layer, and they are transported to the same lip to be combined, and multi-layer shaping is performed, and then cooled and molded, cut, and edged to obtain a three-layer composite glass 1;

[0038] S4, tempering: the three-layer composite glass 1 obtained by the above cooling and molding is sent to a tempering furnace for tempering near the softening temperature of the upper surface glass 11 and the lower surface glass 13 (that is, the tempering temperature is close to the softening point temperature of the upper and lower surface glasses, and lower than the softening point of the middle glass, and the specific tempering temperature is 500-650°C), and then the glass surface temperature is sharply reduced by a strong wind grid, so as to form a compressive stress layer with a depth of more than 100.0μm on the glass surface, thereby increasing the strength of the glass. The wind pressure of the wind grid here can reach 1000-10000Pa, so that a highly flat tempered glass is obtained.

[0039] Example 2

[0040] This embodiment 2 provides a highly flat tempered glass, which is an integrated composite glass structure formed by tempering three layers of laminated glass, including an upper surface glass 11, an intermediate layer glass 12 and a lower surface glass 13 laminated in sequence;

[0041] The total thickness of the high-flatness tempered glass is 1.9 mm, and the thickness of the middle layer glass 12 accounts for about 68.4% of the total thickness, specifically, the thickness of the upper surface glass 11 is 0.3 mm, the thickness of the middle layer glass 12 is 1.3 mm, and the thickness of the lower surface glass 13 is 0.3 mm;

[0042] The intermediate layer of glass 12 plays a supporting role in the glass tempering process. The softening point temperature of the intermediate layer of glass 12 is higher than the softening point temperatures of the upper surface layer of glass 11 and the lower surface layer of glass 13. The tempering molding temperature is near the softening point temperatures of the upper surface layer of glass 11 and the lower surface layer of glass 13.

[0043] The components of the upper surface glass 11 and the lower surface glass 13 are consistent, and they respectively include the following components: SiO2: 70.0wt%; Al2O3: 5.0wt%; CaO: 10.0wt%; MgO: 5.0wt%; Ni2O3: 1.0wt%; K2O: 1.0wt%; CeO2: 0.05wt%; B2O3: 0.9wt%; CuO: 0.05wt%; SrO: 2.0wt% and Na2O: 5.0wt%;

[0044] The intermediate layer glass 12 includes the following components: SiO2: 56.0wt%; Al2O3: 20.0wt%; Na2O: 16.0wt%; CaO: 5.0wt%; MgO: 1.0wt%; K2O: 0.95wt%; CeO2: 0.05wt%; B2O3: 1.0wt%, and the components of the intermediate layer glass 12 satisfy (SiO2+Al2O3+Na2O)≥85.0wt%.

[0045] Example 3

[0046] This embodiment 3 provides a highly flat tempered glass, which is an integrated composite glass structure formed by tempering three layers of laminated glass, and includes an upper surface glass 11, an intermediate layer glass 12 and a lower surface glass 13 laminated in sequence;

[0047] The total thickness of the high-flatness tempered glass is 1.3 mm, and the thickness of the middle layer glass 12 accounts for about 53.8% of the total thickness, specifically, the thickness of the upper surface glass 11 is 0.3 mm, the thickness of the middle layer glass 12 is 0.7 mm, and the thickness of the lower surface glass 13 is 0.3 mm;

[0048] The intermediate layer of glass 12 plays a supporting role in the glass tempering process. The softening point temperature of the intermediate layer of glass 12 is higher than the softening point temperatures of the upper surface layer of glass 11 and the lower surface layer of glass 13. The tempering molding temperature is near the softening point temperatures of the upper surface layer of glass 11 and the lower surface layer of glass 13.

[0049] The components of the upper surface glass 11 and the lower surface glass 13 are consistent, and respectively include the following components: SiO2: 82.0wt%; Al2O3: 3.0wt%; CaO: 7.0wt%; MgO: 3.0wt%; Ni2O3: 0.3wt%; K2O: 0.2wt%; CeO2: 0.1wt%; B2O3: 0.2wt%; CuO: 0.1wt%; SrO: 1.1wt% and Na2O: 3.0wt%;

[0050] The intermediate layer glass 12 includes the following components: SiO2: 68.0wt%; Al2O3: 10.0wt%; Na2O: 9.0wt%; CaO: 8.0wt%; MgO: 4.5wt%; K2O: 0.1wt%; CeO2: 0.2wt%; B2O3: 0.2wt%, and the components of the intermediate layer glass 12 satisfy (SiO2+Al2O3+Na2O)≥85.0wt%.

[0051] Example 4

[0052] The difference between Example 4 and Example 1 is that the total thickness of the high-flatness tempered glass of Example 4 is 1.6 mm, the thickness of the upper surface glass 11 is 0.4 mm, the thickness of the middle layer glass 12 is 0.8 mm, and the thickness of the lower surface glass 13 is 0.4 mm. The rest is the same as Example 1.

[0053] Example 5

[0054] The difference between Example 5 and Example 1 is that the total thickness of the high-flatness tempered glass in Example 5 is 2.0 mm, the thickness of the upper surface glass 11 is 0.55 mm, the thickness of the middle layer glass 12 is 0.9 mm, and the thickness of the lower surface glass 13 is 0.55 mm. The rest is the same as Example 1.

[0055] Comparative Example 1

[0056] Comparative Example 1 is a single-layer glass structure with a thickness of 2.0 mm, and is tempered.

[0057] test:

[0058] The properties of the tempered glasses obtained in Examples 1 to 5 and Comparative Example 1 were tested. The specific test results are shown in the following table:

[0059]

[0060]

[0061] From the test results in the above table, it can be seen that the multi-layer composite glass (tempered glass) provided in Examples 1 to 4 of the present invention has a thickness reduced by 10%, 5%, 35% and 20% respectively compared with the glass of Comparative Example 1 (the weight is also reduced as the thickness is reduced), and the composite glass of the present invention also has strength performance comparable to the thicker and heavier glass of Comparative Example 1; at the same time, compared with the single-layer glass of Comparative Example 1, the multi-layer composite glass (tempered glass) of the present invention has lower warping, which shows that the composite glass provided by the present invention has better flatness.

[0062] The above are preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A highly flat tempered glass, characterized in that: The highly flat tempered glass is an integrated composite glass structure formed by tempering and molding n layers of laminated glass; Among them, the middle layer of glass plays a supporting role in the glass tempering process. The softening point temperature of the middle layer of glass is higher than the softening point temperature of the upper and lower surface glass. The tempering molding temperature is in the softening point temperature range of the upper and lower surface glass. Wherein, n is a positive integer and satisfies n≥3.

2. The highly flat tempered glass according to claim 1, characterized in that: The thickness of the middle layer of glass accounts for 40.0 to 70.0% of the total thickness of the high-flatness tempered glass.

3. A highly flat tempered glass according to claim 1 or 2, characterized in that: The highly flat tempered glass is a composite glass (1) with a three-layer structure, comprising an upper surface layer of glass (11), an intermediate layer of glass (12) and a lower surface layer of glass (13) stacked in sequence; The softening point temperature of the intermediate layer glass (12) is higher than the softening point temperatures of the upper surface layer glass (11) and the lower surface layer glass (13).

4. A highly flat tempered glass according to any one of claims 1 to 3, characterized in that: The components of the upper surface glass and the lower surface glass are consistent, and include the following components respectively: SiO2: 70.0~82.0wt%; Al2O3: 0.1~5.0wt%; CaO: 5.0~10.0wt%; MgO: 1.0~5.0wt%; Ni2O3: 0.1~1.0wt%; K2O: 0~1.0wt%; CeO2: 0~0.2wt%; B2O3: 0~1.0wt%; CuO: 0~0.1wt%; SrO: 0.01~2.0wt% and Na2O: 1.0~5.0wt%.

5. The highly flat tempered glass according to any one of claims 1 to 3, characterized in that: The intermediate layer glass comprises the following components: SiO2: 55.0-68.0wt%; Al2O3: 10.0-20.0wt%; Na2O: 9.0-16.0wt%; CaO: 5.0-9.0wt%; MgO: 1.0-5.0wt%; K2O: 0-1.0wt%; CeO2: 0-0.2wt%; B2O3: 0-1.0wt%; the components of the intermediate layer glass satisfy (SiO2+Al2O3+Na2O)≥85.0wt%.

6. A method for preparing a highly flat tempered glass according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1. Batching: batching the raw materials of the upper surface glass, the middle layer glass and the lower surface glass respectively, and then conveying them to a mixing and stirring machine respectively for uniform stirring and mixing; S2, melting: sending the mixed raw materials into a multi-layer furnace for melting to form three kinds of uniform bubble-free glass liquids respectively; S3, cooling and molding: the three kinds of glass liquid are sent to the distributor at the entrance of the molding pool, the glass liquid after the upper surface glass is melted is distributed to the upper layer, the glass liquid after the middle layer glass is melted is distributed to the middle layer, and the glass liquid after the lower surface glass is melted is distributed to the lower layer, and they are transported to the same lip to merge, and multi-layer shaping is performed, and then cooled and molded; S4, tempering: sending the multi-layer composite glass obtained by the above cooling and forming into a tempering furnace for tempering and forming, thereby obtaining a tempered glass with high flatness.