Composite waterproof breathable film and preparation method thereof
By forming breathable pores on the heavy ion irradiation film and applying waterproof coating material, the problem of uneven pores of the existing waterproof breathable membrane is solved, and better waterproof and breathable performance and pore uniformity are achieved.
Patent Information
- Application Number
- CN202411185221.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The pores of the existing waterproof and breathable membranes are uneven in the air permeable pores, resulting in unsatisfactory waterproof and breathable performance.
The heavy ion irradiation film is used to etch to form breathable pores, and the waterproof coating material is mixed with the polymer solution to form a mixed gel. It is coated on the etched heavy ion irradiation film through a coating machine, so that it is naturally wet to In the pores, a uniform small breathable pore is formed, and a composite waterproof breathable film is prepared by combining a non-woven fabric as a supporting layer.
The uniform distribution of pores is achieved, waterproof and breathable properties are improved, and the functional impairment caused by uneven pores is eliminated. It is easy to process and the waterproof coating performance can be quickly adjusted.
Smart Images

Figure CN119058221A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waterproof breathable membranes, and in particular relates to a composite waterproof breathable membrane and a preparation method thereof. Background Art
[0002] Waterproof breathable membranes are common consumer products in daily life and can be made into packaging bags, diapers, bandages, protective clothing, etc. Most existing waterproof breathable membranes are formed by stretching. For example, inorganic calcium carbonate is used as a pore-forming agent. After mixing with a waterproof high molecular polymer, it is stretched horizontally, longitudinally or biaxially through twin-screw extrusion. The position of the pore-forming agent is used as a defect point. After stretching, a pore structure is formed to achieve a breathable effect. Alternatively, the waterproof coating material is adhered to a structure such as a heavy ion irradiated membrane, and then the heavy ion irradiated membrane is punched to form a waterproof breathable membrane. Both of the above two methods for preparing waterproof breathable membranes have the phenomenon of uneven pores of the air permeable pores, and their waterproof and breathable properties are not ideal. Summary of the invention
[0003] In order to solve the deficiencies in the prior art, the present invention provides a composite waterproof and breathable membrane with better waterproof and breathable performance and a preparation method thereof.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0005] The preparation method of the composite waterproof breathable membrane comprises the following steps:
[0006] Step S1: placing the heavy ion irradiated film into an etching machine for etching;
[0007] Step S2: taking the base layer, and laminating the heavy ion irradiated film etched in step S1 onto the base layer;
[0008] Step S3: dissolving and mixing the waterproof coating material to obtain a mixed gel, and then using a coating machine to coat the mixed gel on the heavy ion irradiated membrane to form a film by a wet process, and then drying and peeling off the base layer to obtain a composite waterproof and breathable membrane;
[0009] Step S4: Using the non-woven fabric as a support layer, pasting it on the composite waterproof breathable membrane prepared in step S3.
[0010] In a preferred embodiment of the present invention, in step S1, the heavy ion irradiation film material used is any one of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyimide (PI) and polyether sulfone (PES).
[0011] In a preferred embodiment of the present invention, in the step S1, the thickness of the heavy ion irradiated film after etching is 3 to 20 μm.
[0012] In a preferred embodiment of the present invention, in step S1, when the heavy ion irradiated film is placed in an etcher for solution etching, the speed of the etcher is 1.0 m / s, the etching solution is 8 mol / L sodium hydroxide solution, and the etching temperature is 80°C.
[0013] In a preferred embodiment of the present invention, in the step S1, a plurality of air holes are formed after the heavy ion irradiation film etching is completed, and the diameter of the air holes is 0.1-10 μm.
[0014] In a preferred embodiment of the present invention, in step S2, the base layer is any one of a release film, a micro-adhesive film or a carrier film.
[0015] In a preferred embodiment of the present invention, in step S3, the waterproof coating material is one or more of polyvinylidene fluoride (PVDF), nylon-66 (PA66) and polyethersulfone (PES).
[0016] In a preferred embodiment of the present invention, in step S3, the temperature of the coating box in the coating machine is 75°C to 105°C.
[0017] In a preferred embodiment of the present invention, in step S3, after the mixed gel is coated on the heavy ion irradiated membrane, the coated heavy ion irradiated membrane is immersed in water for 3 minutes to solidify the mixed gel.
[0018] By adopting the above technical solution, the present invention has the following beneficial effects:
[0019] The present invention adopts the method of first placing the heavy ion irradiated film into an etching machine for etching to form air holes on the heavy ion irradiated film, and then coating the mixed gel prepared by mixing the waterproof coating material with the polymer solution on the heavy ion irradiated film. The mixed gel can naturally infiltrate into the air holes produced by etching, thereby evenly distributing smaller air holes, thereby achieving higher waterproof performance, eliminating poor functionality caused by uneven pores, and achieving better waterproof and air permeability.
[0020] The composite waterproof breathable membrane of the present invention has the following advantages:
[0021] The composite waterproof breathable membrane described in the present invention is a heavy ion irradiated membrane that is chemically etched to form air holes with a diameter of 0.1 to 10 μm and a thickness of 3 to 20 μm. After being compounded with a waterproof coating material such as PVDF, the mixed gel can naturally infiltrate the etched holes through gravity and be evenly distributed in the gaps (air holes generated by chemical etching), forming smaller micron-level air holes on the surface of the irradiated membrane to achieve the purpose of high waterproofness, thereby eliminating the poor functionality of the waterproof breathable membrane caused by uneven pores. The composite waterproof breathable membrane compounding method described in the present invention is that the mixed gel made of PVDF waterproof coating material is coated on the surface of the etched irradiated membrane by a coating machine, the pore distribution is uniform, the processing is convenient, and the performance of the waterproof coating can be quickly adjusted by adjusting the process parameters of the coating machine.
[0022] In summary, the composite waterproof and breathable membrane of the present invention has the advantages of uniform pores and good waterproof and breathable properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart of the method for preparing the composite waterproof breathable membrane of the present invention;
[0024] Figure 2 It is a test result chart of the composite waterproof breathable membrane produced after the specific implementation of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0026] The components of the embodiments of the present invention generally described and shown in the drawings herein may be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention.
[0027] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0028] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0029] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0030] Example 1
[0031] In this embodiment, a method for preparing a composite waterproof breathable membrane is provided. The waterproof breathable pores of the prepared composite waterproof breathable membrane are uniform and have better waterproof and breathable properties.
[0032] like Figure 1 As shown, in one embodiment of the present invention, the method for preparing the composite waterproof breathable membrane of the present invention comprises the following steps:
[0033] Step S1: placing a heavy ion irradiated film into an etching machine for etching, wherein the heavy ion irradiated film material used is any one of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyimide (PI) and polyethersulfone (PES), and the thickness of the heavy ion irradiated film after etching is 3 to 20 μm. After the heavy ion irradiated film is etched, a plurality of air holes are formed, and the diameter of the air holes is 0.1 to 10 μm. Specifically, when the heavy ion irradiated film is placed in the etching machine for solution etching, the speed of the etching machine is 1.0 m / s, the etching solution is 8 mol / L sodium hydroxide solution, and the etching temperature is 80°C;
[0034] Step S2: taking a base layer, and laminating the heavy ion irradiated film etched in step S1 onto the base layer, wherein the base layer is any one of a release film, a micro-adhesive film, or a carrier film;
[0035] Step S3: dissolving and mixing the waterproof coating material to obtain a mixed gel, specifically, taking the waterproof coating material and a polymer solution and then mixing the waterproof coating material and the polymer solution to obtain a mixed gel, and then using a coating machine to coat the mixed gel on the heavy ion irradiated membrane, wet film forming, drying and peeling off the base layer to obtain a composite waterproof breathable membrane, the waterproof coating material is one or more of polyvinylidene fluoride (PVDF), nylon-66 (PA66) and polyethersulfone (PES), specifically, the coating box temperature in the coating machine is 75°C to 105°C, in the step S3, after coating the mixed gel on the heavy ion irradiated membrane, the coated heavy ion irradiated membrane is immersed in water for 3 minutes to solidify the mixed gel, in the present invention, the specific materials of the heavy ion irradiated membrane and the waterproof coating material can be the same or different, after the composite waterproof breathable membrane is obtained, its side can be provided with a double-sided adhesive ring for easy pasting;
[0036] Step S4: Using the non-woven fabric as a support layer, pasting it on the composite waterproof breathable membrane prepared in step S3.
[0037] The invention also discloses a composite waterproof breathable membrane, which is prepared according to the preparation method of the composite waterproof breathable membrane.
[0038] In this embodiment, more detailed and specific data are used for processing and preparation. Specifically, the heavy ion irradiated PET film is placed on an etcher for etching. The etching process parameters are as follows: the concentration of sodium hydroxide is 8 mol / L, the temperature of sodium hydroxide is 80°C, and the speed of the etcher is 1.0 m / s. After the etching is completed, the etched PET film is placed on a coater and coated with a pre-prepared mixed gel of PVDF material. The coating process parameters are as follows: the oven temperature of the coater: 75-105°C, the coating thickness is 27-30 μm, and after the coating is completed, it is soaked in water and specifically soaked in 15°C water for 3 minutes.
[0039] Comparative Example 1
[0040] This comparative example adopts the same preparation method as Example 1, but the specific preparation values are different. Specifically, the heavy ion irradiated PET film is placed on an etcher for etching, and the etching process parameters are as follows: the concentration of sodium hydroxide is 8 mol / L, the temperature of sodium hydroxide is 80°C, and the speed of the etcher is 1 m / s. After etching, the etched PET film is placed on a coater and coated with a pre-prepared PVDF mixed gel. The coating process parameters are as follows: coating machine oven temperature: 75-105°C, the coating thickness is 15-17 μm, and after coating, it is soaked in 15°C water for 3 minutes.
[0041] like Figure 2As shown, the difference between this comparative example and Example 1 is that the coating thickness is different. In Example 1, when the immersion conditions are room temperature and immersion in 15°C water temperature for 3 minutes, the air permeability is better when immersed in 15°C water temperature for 3 minutes. In Comparative Example 1, when the immersion conditions are also room temperature and immersion in 15°C water temperature for 3 minutes, the air permeability is better when immersed in 15°C water temperature for 3 minutes.
[0042] Comparative Example 2
[0043] This comparative example adopts the same preparation method as Example 1, and the specific preparation values are different. Specifically, the heavy ion irradiated PET film is placed on an etcher for etching, and the etching process parameters are as follows: the concentration of sodium hydroxide is 8 mol / L, the temperature of sodium hydroxide is 80°C, and the speed of the etcher is 1 m / s. After the etching is completed, the etched PET film is placed on a coater and coated with a pre-prepared PVDF mixed gel. The coating process parameters are as follows: coating machine oven temperature: 75-105°C, the coating thickness is 15-17μm, and after the coating is completed, it is soaked in 5°C water for 3 minutes.
[0044] After completing Example 1 and Comparative Example 1 and Comparative Example 2, the composite waterproof breathable membrane was prepared, and the composite waterproof breathable membrane was tested. The test comparison results are specifically referred to Figure 2 The tests include pore size measurement, air permeability measurement, waterproof performance test, thickness test, audio performance test, etc. The pore size measurement is to place the etched PET film sample on a microscope and measure its pore size at ×3000 times. The air permeability measurement is to place the composite waterproof and breathable membrane obtained after coating on a leak detector and test its air permeability under a pressure of 7KPA. The waterproof performance test is to place the composite waterproof and breathable membrane obtained after coating on a leak detector, and inject water into the test tube connected between the leak detector and the test fixture. At 500KPA, test whether it leaks for a period of time. The thickness test is to measure the thickness of the composite waterproof and breathable membrane obtained after coating with a micrometer. The audio performance test is tested on an audio tester, and the membrane material is analyzed by the DB value of audio distortion.
[0045] Figure 2 The "8 passed 2" means that in the water pressure test, 2 out of 8 test samples passed. Figure 2 By comparison, when immersed in 5°C water for 3 minutes and the coating thickness is 15-17 μm, more composite waterproof breathable membranes of the present invention that are immersed in 5°C water for 3 minutes to complete solidification pass the waterproof test than those immersed in room temperature to complete solidification. The composite waterproof breathable membrane of the present invention has better waterproof and breathable properties.
[0046] Immersion precipitation phase separation is the most common method for preparing PVDF membranes. PVDF is a semi-crystalline polymer that can form a uniform solution with many high-boiling point extreme solvents at room temperature. The polymer solution is then immersed in a non-solvent coagulation bath such as water, alcohol, and ketone. At this time, the solvent in the polymer solution diffuses into the non-solvent, while the non-solvent polymer diffuses to form a kinetic diffusion process. As the diffusion continues, the system undergoes thermodynamic liquid-liquid phase separation, and PVDF membranes of different morphologies and structures are formed through phase transformation.
[0047] In the process of preparing PVDF membrane by immersion precipitation method, the solvent, coagulation bath composition, coagulation bath temperature and evaporation time have a great influence on the membrane structure and performance. It is generally believed that the weaker the interaction between the polymer and the solvent, the faster the precipitation rate of the polymer. The finger-like pores formed by polymerization into solvents, the study found that dimethylamide as solvent forms short finger-like pores, and many dispersed spherical polymer aggregates appear, DMAc, tetramethyl urea, and trimethyl phosphate as solvents form large voids, methyl pyrrolidone and methyl sulfoxide as solvents form wide and long finger-like pores, hexamethylphosphoric acid amide as solvent forms short pores and dispersed holes, and triethyl phosphate as solvent forms a honeycomb structure without voids.
[0048] The heavy ion irradiated membrane is used as the skeleton and composited with PVDF and other materials as the waterproof coating. After chemical etching, the ion irradiated membrane forms air pores of 0.1 to 10 μm, and then PVDF coating is coated on it to form a waterproof and breathable membrane composite material. The waterproof and breathable material with the heavy ion irradiated substrate as the skeleton structure solves the problems of waterproof and breathable performance stability, poor consistency, and unstable quality of the waterproof and breathable membrane materials produced by the existing technology with e-PTFE as the main material. The waterproof coating is composited with the irradiated membrane material to improve the problems of large membrane thickness and uneven gaps, and realize the waterproof and breathable function of the membrane material.
[0049] The micropore density in the present invention is controllable and quantifiable. The pore density of the micropores can be controlled by controlling the intensity of the heavy ion beam emitted by the accelerator and the running speed of the irradiated object. The pore density can reach 8,000,000 per square centimeter. The pore size of the micropores is controllable. The polymer membrane material is bombarded by high-energy heavy ions to break its molecular long chain, and then the etching solution forms micropores at the break. The pore size from nanometer level to micrometer level can be accurately achieved by controlling the concentration, temperature and membrane running speed of the etching solution. The micropores of the present invention are regular cylindrical holes, which can meet the dust and water resistance level requirements of various products. The air permeability of the present invention is stable. The PTFE microporous stretched membrane currently on the market adopts unidirectional stretching or bidirectional stretching, so the air permeability values of different regions have obvious deviations, which can reach more than 20%. However, due to its unique pore-forming process, and the micropore density and pore size are accurately controllable, the air permeability values of different regions of the present invention are very stable, and the deviation value is less than 10%.
[0050] This embodiment does not impose any formal limitation on the shape, material, structure, etc. of the present invention. Any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a composite waterproof breathable membrane, characterized in that: The following steps are involved: Step S1: placing the heavy ion irradiated film into an etching machine for etching; Step S2: taking the base layer, and laminating the heavy ion irradiated film etched in step S1 onto the base layer; Step S3: dissolving and mixing the waterproof coating material to obtain a mixed gel, and then using a coating machine to coat the mixed gel on the heavy ion irradiated membrane to form a film by a wet process, and then drying and peeling off the base layer to obtain a composite waterproof and breathable membrane; Step S4: Using the non-woven fabric as a support layer, pasting it on the composite waterproof breathable membrane prepared in step S3.
2. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In the step S1, the heavy ion irradiation film material used is any one of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyimide (PI) and polyether sulfone (PES).
3. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In the step S1, the thickness of the heavy ion irradiated film after etching is 3 to 20 μm.
4. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In the step S1, when the heavy ion irradiated film is placed in an etcher for solution etching, the speed of the etcher is 1.0 m / s, the etching solution is 8 mol / L sodium hydroxide solution, and the etching temperature is 80°C.
5. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In the step S1, a plurality of vent holes are formed after the heavy ion irradiation film is etched, and the diameter of the vent holes is 0.1-10 μm.
6. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In the step S2, the base layer is any one of a release film, a micro-adhesive film or a carrier film.
7. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In step S3, the waterproof coating material is one or more of polyvinylidene fluoride (PVDF), nylon-66 (PA66) and polyethersulfone (PES).
8. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In the step S3, the temperature of the coating box in the coating machine is 75°C to 105°C.
9. The method for preparing a composite waterproof breathable membrane according to claim 1, characterized in that: In the step S3, after the mixed gel is coated on the heavy ion irradiated membrane, the coated heavy ion irradiated membrane is immersed in water for 3 minutes to solidify the mixed gel.
10. Composite waterproof breathable membrane, characterized by: The composite waterproof breathable membrane is prepared according to the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of water-proof oil-proof breathable film with super-amphiphobic function
CN113248776A
Preparation method and application of waterproof breathable film
CN116903907A
Cited By
Preparation method of fluoride-free waterproof breathable film based on irradiation technology
CN119505361A
Preparation method of waterproof breathable film and waterproof breathable film
CN119639046A
Preparation method of waterproof and breathable film and waterproof and breathable film
CN119639046B