Molybdenum ion doped lithium manganese iron phosphate positive electrode material and preparation method and application thereof

Through the preparation of molybdenum ion-doped lithium manganese iron phosphate positive electrode material, the problems of fast capacity attenuation and poor rate performance of olivine-type LiMn1-xFexPO4 positive electrode material are solved, and the energy density and service life of lithium batteries are improved, and the preparation method is simple. , low cost, suitable for large-scale production.

CN119059504APending Publication Date: 2024-12-03CHINA UNIV OF GEOSCIENCES (WUHAN)

Patent Information

Application Number
CN202411174129.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing olivine-type LiMn1-xFexPO4 positive electrode material has problems of fast capacity attenuation and poor rate performance, which limits its practical application in lithium-ion batteries.

Method used

The preparation method of the lithium manganese iron phosphate positive electrode material doped by molybdenum ion includes dissolving manganese salt, ferrous salt, ammonium dihydrogen phosphate and glucose in deionized water, adding lithium salt and molybdenum oxide, stirring and ball milling, Spray drying and calcined in a nitrogen atmosphere to form a porous microsphere material with a carbon coating on the surface to improve electrochemical properties.

Benefits of technology

It improves ionic conductivity and cycling stability, delays harmful phase change during the charging stage, and improves the energy density and service life of lithium batteries. At the same time, the preparation method is simple, low-cost and can be produced on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059504A_ABST
    Figure CN119059504A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of positive electrode materials, in particular to a molybdenum ion doped lithium manganese iron phosphate positive electrode material and a preparation method and application thereof. The preparation method comprises the following steps: A) dissolving manganese salt, ferrous salt or ferric salt, ammonium dihydrogen phosphate or ammonium phosphate and glucose in deionized water to obtain a mixed solution; slowly adding a lithium salt and molybdenum oxide into the mixed solution, and stirring on a stirrer for one hour at normal temperature to obtain a lithium manganese iron phosphate precursor B) transferring the precursor 1 into a ball milling tank, and carrying out ball milling for a period of time to obtain lithium manganese iron phosphate slurry; c) further sanding the lithium manganese iron phosphate slurry obtained in the step B); and D) carrying out spray drying on the lithium manganese iron phosphate slurry obtained in the step C), and calcining to obtain the molybdenum ion doped lithium manganese iron phosphate positive electrode material. The molybdenum ion doped lithium manganese iron phosphate positive electrode material prepared by the invention can improve the ionic conductivity and improve the excellent capacity and cycling stability of lithium manganese iron phosphate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of positive electrode materials, and in particular to a molybdenum ion-doped lithium manganese iron phosphate positive electrode material and a preparation method and application thereof. Background Art

[0002] Among all kinds of lithium-ion battery cathode materials, olivine-type LiFePO4 cathode materials have attracted widespread attention due to their low cost, long cycle stability and high safety. However, it is limited by a lower voltage platform (≈3.4V), resulting in low energy density. Another olivine-type LiMnPO4 similar to LiFePO4, although it has a higher voltage platform and a theoretical energy density of ≈701Wh kg-1, has extremely low intrinsic electronic conductivity, as well as extremely poor cycle stability and rate performance caused by the dissolution of Mn and the Jahn-Teller distortion effect during the cycle, which limits its further practical application.

[0003] Olive-type LiMn1-xFexPO4 (LMFP) is a new type of material that combines the advantages of LiFePO4 and LiMnPO4, which can effectively improve their intrinsic defects and increase their conductivity. However, it still has technical problems such as fast capacity decay and poor rate performance. Summary of the invention

[0004] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide a molybdenum ion-doped lithium manganese iron phosphate positive electrode material and a preparation method and application thereof.

[0005] A method for preparing a molybdenum ion-doped lithium manganese iron phosphate positive electrode material of the present invention comprises the following steps:

[0006] A) dissolving a manganese salt, a ferrous salt or a ferric salt, ammonium dihydrogen phosphate or ammonium phosphate, and glucose in deionized water to obtain a mixed solution; then slowly adding a lithium salt and molybdenum oxide to the mixed solution, and then stirring the mixture on a stirrer at room temperature for one hour to obtain a lithium iron manganese phosphate precursor;

[0007] B) transferring the precursor 1 to a ball mill and ball milling for a period of time to obtain lithium iron manganese phosphate slurry;

[0008] C) further sand grinding the lithium iron manganese phosphate slurry obtained in B);

[0009] D) spray-drying the lithium iron manganese phosphate slurry obtained in C) and then calcining it to obtain a molybdenum ion-doped lithium iron manganese phosphate positive electrode material.

[0010] Furthermore, in step A), in the mixed solution, the molar ratio of manganese, iron, phosphorus, lithium, molybdenum and glucose is 0.5-1:0.5-1:1:1-1.2:0.01-0.02:0.1-0.2.

[0011] Furthermore, in the step A), the salt containing manganese element is manganese oxalate or manganese hydrogen phosphate, the ferrous salt is ferrous oxalate, the ferric salt is ferric phosphate, and the lithium salt is lithium carbonate or lithium dihydrogen phosphate.

[0012] Furthermore, the dissolution temperature is 90°C-95°C.

[0013] Furthermore, in the step B), the ball-to-material ratio is 1:1.5-2, the ball milling is performed for 5-6 hours, and the rotation speed is 400-450 r / min.

[0014] Furthermore, in step D), the spray drying conditions are as follows: an inlet temperature of 150° C.-200° C., a feed rate of 10-20 mL / min, and a fan frequency of 30-40 Hz.

[0015] Furthermore, in the step D), the calcination atmosphere is nitrogen, the powder calcination temperature is 650° C.-700° C., the heating rate is 1-5° C. / min, and the calcination time is 6-8 h.

[0016] A molybdenum ion-doped lithium manganese iron phosphate positive electrode material prepared by the above-mentioned preparation method.

[0017] An application of the molybdenum ion-doped lithium manganese iron phosphate positive electrode material as described above in a lithium battery.

[0018] The molybdenum ion doped lithium manganese iron phosphate positive electrode material prepared by the present invention is porous microspheres, and a carbon coating is constructed on the surface and molybdenum element is doped to change its electrochemical properties. Mo ions with a larger radius are doped at the Fe / Mn position to shorten the Li-O bonding, reduce the gap position in the octahedral LiO6, connect the MO octahedron and the PO tetrahedron, and the PO covalent bond will also be appropriately weakened. At the same time, molybdenum element doping can expand the interlayer spacing, improve the rate performance of the modified sample, and delay the harmful phase change in the charging stage.

[0019] The molybdenum ion-doped lithium manganese iron phosphate positive electrode material prepared by the present invention can improve ion conductivity, improve the excellent capacity and cycle stability of lithium manganese iron phosphate, and can be applied to lithium ion batteries to improve the energy density and service life of lithium batteries; the preparation method is simple, operability is strong, cost is low, raw materials are easily available, conditions are mild, and energy consumption is extremely low; the main production process can be automated and unattended, and large-scale production can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 XRD diagrams of the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 1 and the platinum ion-doped lithium iron manganese phosphate positive electrode material prepared in Example 1 of the present invention;

[0021] Figure 2This is a FESEM image of the molybdenum ion-doped lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention;

[0022] Figure 3 Capacity cycle diagram of a half-cell assembled with the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 1 and the platinum ion-doped lithium iron manganese phosphate positive electrode material prepared in Example 1 of the present invention at 1C;

[0023] Figure 4 Typical discharge capacity curves of the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 1 and the platinum ion-doped lithium iron manganese phosphate positive electrode material prepared in Example 1 of the present invention at a current density of 5C within a voltage range of 2.2-4.5V;

[0024] Figure 5 The rate performance diagram of the half-cell assembled with the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 1 and the platinum ion-doped lithium iron manganese phosphate positive electrode material prepared in Examples 1-3 of the present invention at 0.2C-10C;

[0025] Figure 6 Electrochemical impedance diagrams of the sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the molybdenum ion-doped lithium iron manganese phosphate positive electrode material prepared in Example 1 of the present invention and lithium iron manganese phosphate. DETAILED DESCRIPTION

[0026] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0027] Example 1

[0028] A) 14.296 g (0.1 mol) of manganese oxalate (relative molecular mass of 142.96), 16.92 g (0.094 mol) of ferrous oxalate (relative molecular mass of 143.86), 23 g (0.2 mol) of diammonium phosphate (relative molecular mass of 115), 18 g (0.1 mol) of glucose (relative molecular mass of 180), 7.389 g (0.1 mol) of lithium carbonate (relative molecular mass of 74), and 0.29 g of molybdenum oxide (relative molecular mass of 144) were weighed; manganese oxalate, ferrous oxalate, diammonium phosphate, and glucose were dissolved in 90° C. deionized water to obtain a mixed solution 1; lithium carbonate and molybdenum oxide were slowly added to the mixed solution 1 to obtain a mixed solution 2, and then stirred on a stirrer at room temperature for one hour to obtain a lithium iron manganese phosphate precursor 1;

[0029] B) Precursor 1 and glucose were mixed in a molar ratio of 1:0.1, added to deionized water, stirred at 60° C. for 1 h, and then transferred to a ball mill, zirconium oxide beads were selected, the solid content was controlled at about 60%, the ball-to-material ratio was 1:2, and ball milling was performed for 5 hours at a speed of 400 rpm to obtain lithium iron manganese phosphate slurry;

[0030] C) further sand grinding the lithium iron manganese phosphate slurry obtained in B);

[0031] D) spray drying the obtained lithium iron manganese phosphate slurry into balls; the spray drying conditions are an inlet temperature of 150°C, a feed rate of 10 mL / min, and a fan frequency of 30 Hz; the lithium iron manganese phosphate powder collected by spray drying is calcined at 650°C and heated in a N2 atmosphere at a heating rate of 5°C / min for 6 hours to obtain a lithium iron manganese phosphate positive electrode material.

[0032] Example 2

[0033] A) 14.296 g (0.1 mol) of manganese oxalate (relative molecular mass of 142.96), 16.92 g (0.094 mol) of ferrous oxalate (relative molecular mass of 143.86), 23 g (0.2 mol) of diammonium phosphate (relative molecular mass of 115), 18 g (0.1 mol) of glucose (relative molecular mass of 180), 7.389 g (0.1 mol) of lithium carbonate (relative molecular mass of 74), and 0.43 g of molybdenum oxide (relative molecular mass of 144) were weighed; manganese oxalate, ferrous oxalate, diammonium phosphate, and glucose were dissolved in 90° C. deionized water to obtain a mixed solution 1; lithium carbonate and molybdenum oxide were slowly added to the mixed solution 1 to obtain a mixed solution 2, and then stirred on a stirrer at room temperature for one hour to obtain a lithium iron manganese phosphate precursor 1;

[0034] B) Precursor 1 was added to deionized water, stirred at 60° C. for 1 h, and then transferred to a ball mill, zirconium oxide beads were selected, the solid content was controlled at about 60%, the ball-to-material ratio was 1:2, and the ball milling was performed for 5 hours at a speed of 400 rpm to obtain lithium iron manganese phosphate slurry;

[0035] C) further sand grinding the lithium iron manganese phosphate slurry obtained in B);

[0036] D) spray drying the obtained lithium iron manganese phosphate slurry into balls; the spray drying conditions are an inlet temperature of 150°C, a feed rate of 10 mL / min, and a fan frequency of 30 Hz. The lithium iron manganese phosphate powder collected by spray drying is calcined at 650°C and heated in a N2 atmosphere at a heating rate of 5°C / min for 6 hours to obtain a lithium iron manganese phosphate positive electrode material.

[0037] Example 3

[0038] A) 14.296 g (0.1 mol) of manganese oxalate (relative molecular mass of 142.96), 16.92 g (0.094 mol) of ferrous oxalate (relative molecular mass of 143.86), 23 g (0.2 mol) of diammonium phosphate (relative molecular mass of 115), 18 g (0.1 mol) of glucose (relative molecular mass of 180), 7.389 g (0.1 mol) of lithium carbonate (relative molecular mass of 74), and 0.58 g of molybdenum oxide (relative molecular mass of 144) were weighed; manganese oxalate, ferrous oxalate, diammonium phosphate, and glucose were dissolved in 90° C. deionized water to obtain a mixed solution 1; lithium carbonate and molybdenum oxide were slowly added to the mixed solution 1 to obtain a mixed solution 2, and then stirred on a stirrer at room temperature for one hour to obtain a lithium iron manganese phosphate precursor 1;

[0039] B) adding the precursor to deionized water, stirring at 60° C. for 1 h, and then transferring to a ball mill, selecting zirconium oxide beads, controlling the solid content to about 60%, the ball-to-material ratio to 1:2, and ball milling for 5 hours at a speed of 400 rpm to obtain lithium iron manganese phosphate slurry;

[0040] C) further sand grinding the lithium iron manganese phosphate slurry obtained in B);

[0041] D) spray drying the obtained lithium iron manganese phosphate slurry into balls; the spray drying conditions are an inlet temperature of 150°C, a feed rate of 10 mL / min, and a fan frequency of 30 Hz. The lithium iron manganese phosphate powder collected by spray drying is calcined at 700°C and heated in a N2 atmosphere at a heating rate of 5°C / min for 6 hours to obtain a lithium iron manganese phosphate positive electrode material.

[0042] Comparative Example 1

[0043] A) 14.296 g (0.1 mol) of manganese oxalate (relative molecular mass of 142.96), 16.92 g (0.094 mol) of ferrous oxalate (relative molecular mass of 143.86), 23 g (0.2 mol) of diammonium phosphate (relative molecular mass of 115), 18 g (0.1 mol) of glucose (relative molecular mass of 180), and 7.389 g (0.1 mol) of lithium carbonate (relative molecular mass of 74) were weighed; manganese oxalate, ferrous oxalate, diammonium phosphate, and glucose were dissolved in 90° C. deionized water to obtain a mixed solution 1; lithium carbonate was then slowly added to the mixed solution 1 to obtain a mixed solution 2, and then stirred on a stirrer at room temperature for one hour to obtain a lithium iron manganese phosphate precursor 1;

[0044] B) adding the precursor to deionized water, stirring at 60° C. for 1 h, and then transferring to a ball mill, selecting zirconium oxide beads, controlling the solid content to about 60%, the ball-to-material ratio to 1:2, and ball milling for 5 hours at a speed of 400 rpm to obtain lithium iron manganese phosphate slurry;

[0045] C) further sand grinding the lithium iron manganese phosphate slurry obtained in B);

[0046] D) spray drying the obtained lithium iron manganese phosphate slurry into balls. The spray drying conditions are an inlet temperature of 150°C, a feed rate of 10 mL / min, and a fan frequency of 30 Hz. Finally, the lithium iron manganese phosphate powder collected by spray drying is calcined at 650°C and heated in a N2 atmosphere at a heating rate of 5°C / min for 6 hours to obtain a lithium iron manganese phosphate positive electrode material.

[0047] The difference between Comparative Example 1 and Example 2 is that molybdenum oxide is not added during the synthesis stage.

[0048] The Mo metal-doped lithium manganese iron phosphate composite material prepared in Example 2 was assembled into a half-cell, and the active positive electrode material, acetylene black and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 8:1:1, and then the mixture was dispersed in N-methyl-2-pyrrolidone (NMP) for 12 hours using a magnetic stirrer to form a uniform slurry, after which the slurry was coated on aluminum foil and finally dried in a vacuum oven at 100°C for 22 hours to remove NMP. The electrode sheet was prepared by cutting the aluminum foil into a disc with a diameter of 10 mm, and the mass loading of the cut electrode sheet was 2 to 3 mg cm -2 CR2032 button cells were assembled in an argon glove box. LI metal sheets and PP separators were used as counter electrodes and separators, respectively. The electrolyte was 1 mol L dissolved in ethylene carbonate / diethyl carbonate (EC / DEC) (volume ratio = 1:1). -1 LiPF6.

[0049] The Mo metal-doped lithium manganese iron phosphate composite electrode material obtained by the above-mentioned method for preparing a metal-doped lithium manganese iron phosphate composite electrode material is a LMFP / C-Mo composite electrode material.

[0050] Figure 1 The XRD patterns of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 and the molybdenum ion-doped lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention are compared with the standard card, and the correspondence with the standard card is good, confirming that the product prepared in Comparative Example 1 is LMFP / C, and the product prepared in Example 2 is LMFP / C-Mo.

[0051] Figure 2 This is a FESEM image of the molybdenum ion-doped lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention; it can be seen that the LMFP / C-Mo material is in the shape of microspheres with a diameter of 10-15 μm.

[0052] Figure 3This is a nitrogen adsorption-desorption curve of the molybdenum ion-doped lithium manganese iron phosphate positive electrode material prepared in Example 2; it can be seen that the LMFP / C-Mo material has a large specific surface area and abundant internal pores.

[0053] Figure 4 The lithium manganese iron phosphate positive electrode material prepared in comparative example 1 and the LMFP / C-Mo material prepared in example 1 of the present invention are within the voltage range of 2.2-4.5V, 5C (1C = 170mAh·g -1 ) The typical discharge capacity curve under current density. It can be seen from the figure that the discharge capacity of LMFP / C-0.01Mo (X = 0.01) positive electrode material is 118mAh g -1 , the capacity retention rate is 98% after 400 cycles.

[0054] Figure 5 The typical discharge capacity curves of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 and the LMFP / C-Mo material prepared in Examples 1-3 of the present invention at different current densities of 0.1C-10C in the voltage range of 2.2-4.5V. As can be seen from the figure, the discharge capacity of the LMFP / C-0.005Mo (X=0.005) positive electrode material at a current density of 0.1C is 150mAh·g -1 The discharge capacity at 10C current density is 65 mAh g -1 .

[0055] The discharge capacity of LMFP / C-0.01Mo (X=0.01) cathode material at 0.1C current density is 156mAh·g -1 The discharge capacity at 10C current density is 89 mAh g -1 .

[0056] The discharge capacity of LMFP / C-0.015Mo (X=0.015) cathode material at 0.1C current density is 148 mAh g -1 The discharge capacity at 10C current density is 63 mAh g -1 .

[0057] Figure 6 The electrochemical impedance spectra of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 and the LMFP / C-0.01Mo electrode prepared in Example 2 of the present invention in the range of 100000-0.01Hz show that the LMFP / C-0.01Mo electrode has a smaller electrochemical impedance, which proves that the doping of molybdenum ions effectively improves the conductivity of the lithium manganese iron phosphate.

[0058] For matters not mentioned above, the prior art applies.

[0059] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a molybdenum ion-doped lithium manganese iron phosphate positive electrode material, characterized in that: The steps include: A) dissolving a manganese salt, a ferrous salt or a ferric salt, ammonium dihydrogen phosphate or ammonium phosphate, and glucose in deionized water to obtain a mixed solution; then slowly adding a lithium salt and molybdenum oxide to the mixed solution, and then stirring the mixture on a stirrer at room temperature for one hour to obtain a lithium iron manganese phosphate precursor; B) transferring the precursor 1 to a ball mill and ball milling for a period of time to obtain lithium iron manganese phosphate slurry; C) further sand grinding the lithium iron manganese phosphate slurry obtained in B); D) spray-drying the lithium iron manganese phosphate slurry obtained in C) and then calcining it to obtain a molybdenum ion-doped lithium iron manganese phosphate positive electrode material.

2. The preparation method according to claim 1, characterized in that: In step A), in the mixed solution, the molar ratio of manganese, iron, phosphorus, lithium, molybdenum and glucose is 0.5-1:0.5-1:1:1-1.2:0.01-0.02:0.1-0.

2.

3. The preparation method according to claim 1, characterized in that: In the step A), the salt containing manganese element is manganese oxalate or manganese hydrogen phosphate, the ferrous salt is ferrous oxalate, the ferric salt is ferric phosphate, and the lithium salt is lithium carbonate or lithium dihydrogen phosphate.

4. The preparation method according to claim 1, characterized in that: The dissolving temperature is 90℃-95℃.

5. The preparation method according to claim 1, characterized in that: In the step B), the ball-to-material ratio is 1:1.5-2, the ball milling is performed for 5-6 hours, and the rotation speed is 400-450 r / min.

6. The preparation method according to claim 1, characterized in that: In step D), the spray drying conditions are as follows: an inlet temperature of 150° C.-200° C., a feed rate of 10-20 mL / min, and a fan frequency of 30-40 Hz.

7. The preparation method according to claim 1, characterized in that: In the step D), the calcination atmosphere is nitrogen, the powder calcination temperature is 650° C.-700° C., the heating rate is 1-5° C. / min, and the calcination time is 6-8 hours.

8. A molybdenum ion-doped lithium manganese iron phosphate positive electrode material prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the molybdenum ion-doped lithium manganese iron phosphate positive electrode material as claimed in claim 8 in a lithium battery.

Citation Information

Patent Citations

  • Rapid preparation method of spherical lithium iron manganese phosphate positive electrode material

    CN116216685A

  • Doped lithium iron manganese phosphate positive electrode material, preparation method thereof, positive electrode plate containing doped lithium iron manganese phosphate positive electrode material, and lithium ion battery containing doped lithium iron manganese phosphate positive electrode material

    CN116741987A

  • Preparation method of nano high-activity lithium manganese iron phosphate positive electrode material

    CN117069084A

  • Composite doped modified lithium manganese iron phosphate positive electrode material as well as preparation method and application thereof

    CN117174853A

  • Preparation method of doped lithium iron manganese phosphate positive electrode material

    CN117886289A

Cited By

  • Lithium manganese iron phosphate positive electrode material based on multi-dimensional conductive network construction and grain boundary passivation and preparation method of lithium manganese iron phosphate positive electrode material

    CN121247758A

  • Positive electrode active material, electrode, and battery

    JP2026100782A