Multi-walled carbon nanotube dispersion liquid as well as preparation method and application thereof

Through the use of swelling and expansion treatment combined with the use of surfactant, the problem of easy breakage of multi-wall carbon nanotubes during dispersion is solved, and an efficient multi-wall carbon nanotube dispersion is prepared, which improves the conductivity and battery capacity of ion batteries , reduces costs.

CN119059515AActive Publication Date: 2024-12-03YONGJIANG LAB
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411555862.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
2044-11-04

AI Technical Summary

Technical Problem

Multi-walled carbon nanotubes are prone to break during dispersion, resulting in poor conductivity in ion batteries and unable to effectively wrap active substance particles, increasing the cost of the battery.

Method used

Through swelling and expansion treatment, the multi-wall carbon nanotube powder is expanded and dispersed, and the dispersion effect is significantly improved by combining non-thickening surfactants, and the viscosity of the predispersion liquid is increased through thickening surfactants, reducing free movement between molecules , avoid breakage, and prepare a uniform and stable multi-wall carbon nanotube dispersion.

Benefits of technology

The dispersion and stability of multi-wall carbon nanotubes are improved, the conductivity and battery capacity of ion batteries are enhanced, and the cost of the battery is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059515A_ABST
    Figure CN119059515A_ABST
Patent Text Reader

Abstract

The invention relates to a multiwalled carbon nanotube dispersion liquid and a preparation method and application thereof. The preparation method comprises the following steps: carrying out swelling treatment on multiwalled carbon nanotube powder, and separating to obtain a first intermediate product; mixing the first intermediate product with manganese dioxide and a non-thickening surfactant, then adding hydrogen peroxide for expansion treatment, and separating to obtain a second intermediate product; the second intermediate product is mixed with a thickening type surfactant and a solvent to form a pre-dispersion liquid, then the pre-dispersion liquid is subjected to at least two times of dispersion treatment, the multi-walled carbon nanotube dispersion liquid is obtained, and the mass fraction of the second intermediate product in the pre-dispersion liquid is smaller than 1.5%. According to the preparation method, the problem that the multi-walled carbon nanotubes are easy to break in the dispersion process can be solved, the multi-walled carbon nanotubes in the obtained dispersion liquid are uniformly dispersed and high in stability, and the conductivity and the capacity of the battery can be effectively improved when the dispersion liquid is applied to the ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon nanotubes, and in particular to a multi-walled carbon nanotube dispersion liquid and a preparation method and application thereof. Background Art

[0002] Multi-walled carbon nanotubes and single-walled carbon nanotubes have the same graphitized structure on the surface. However, compared with flexible single-walled carbon nanotubes, multi-walled carbon nanotubes have more walls and a larger diameter, which makes them more rigid and brittle. They are easy to break during the dispersion process and have large defects. As a result, when they are used as a conductive agent in ion batteries, they cannot wrap the entire active material particles well, which is not conducive to building a good conductive network. At the same time, the "needle effect" in the silicon-based negative electrode causes GPa-level compressive stress on the carbon tubes during the cycle, which will puncture the SEI and the coating. Therefore, single-walled carbon nanotubes are currently mainly used as conductive agents in ion batteries.

[0003] However, compared with single-walled carbon nanotubes, multi-walled carbon nanotube powder has a higher yield. If the brittleness of multi-walled carbon nanotubes can be overcome during the dispersion process and their breakage can be avoided to the greatest extent, the cost of ion batteries can be greatly reduced. Summary of the invention

[0004] Based on this, it is necessary to provide a multi-walled carbon nanotube dispersion and a preparation method and application thereof to address the above problems. The preparation method can overcome the problem that multi-walled carbon nanotubes are easily broken during the dispersion process, and the multi-walled carbon nanotubes in the obtained dispersion are evenly dispersed and highly stable. Applying it to ion batteries can effectively improve the conductivity and capacity of the batteries.

[0005] A method for preparing a multi-walled carbon nanotube dispersion comprises the following steps: Swelling the multi-walled carbon nanotube powder to obtain a first intermediate product; The first intermediate product is mixed with manganese dioxide and a non-thickening surfactant, and then hydrogen peroxide is added to perform expansion treatment, and a second intermediate product is obtained by separation; The second intermediate product is mixed with a thickening surfactant and a solvent to form a pre-dispersion liquid, and then the pre-dispersion liquid is subjected to at least a secondary dispersion treatment to obtain a multi-walled carbon nanotube dispersion liquid, wherein the mass fraction of the second intermediate product in the pre-dispersion liquid is less than 1.5%.

[0006] In one embodiment, in the step of subjecting the multi-walled carbon nanotube powder to swelling treatment, the multi-walled carbon nanotube powder is mixed with an acid to perform the swelling treatment.

[0007] In one embodiment, the step of mixing the multi-walled carbon nanotube powder with an acid for swelling treatment satisfies at least one of the following conditions: (1) The acid is at least one selected from chlorosulfonic acid, concentrated nitric acid, concentrated sulfuric acid, and concentrated hydrochloric acid; (2) The mass ratio of the acid to the multi-walled carbon nanotube powder is 10:1-100:1; (3) The temperature of the swelling treatment is 10°C-60°C, and the time is 15min-8h.

[0008] In one embodiment, in the step of adding hydrogen peroxide for expansion treatment, the hydrogen peroxide is added in batches.

[0009] In one embodiment, the expansion step further satisfies at least one of the following conditions: (1) The mass ratio of the hydrogen peroxide to the manganese dioxide is 10:1-50:1; (2) The mass ratio of the hydrogen peroxide to the multi-walled carbon nanotube powder is 5:1-50:1; (3) The expansion treatment is carried out at a temperature of 10°C to 85°C and for a time of 15 minutes to 8 hours; (4) The mass ratio of the non-thickening surfactant to the multi-walled carbon nanotube powder is 1:10-10:10; (5) The non-thickening surfactant is selected from at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium polystyrene sulfonate, lithium polystyrene sulfonate, sodium lignin sulfonate, alkali lignin, polyvinyl pyrrolidone or sodium dodecyl sulfate.

[0010] In one embodiment, the pre-dispersion liquid further satisfies at least one of the following conditions: (1) The mass ratio of the thickening surfactant to the multi-walled carbon nanotube powder is 2.5:10-15:10; (2) The thickening surfactant is at least one selected from sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium hexametaphosphate or sodium alginate; (3) The solvent is selected from water.

[0011] In one embodiment, the dispersion treatment method is selected from air flow grinding, emulsification shearing, colloid milling, ball milling, ultrasonic crushing, high-pressure homogenization or sand milling.

[0012] In one embodiment, the pre-dispersion liquid is subjected to a primary dispersion treatment and a secondary dispersion treatment in sequence, wherein the primary dispersion treatment is selected from at least one of air flow crushing, emulsification shearing, colloid milling or ball milling, and the secondary dispersion treatment is selected from at least one of ultrasonic crushing, high-pressure homogenization or sand milling.

[0013] The present invention also provides a multi-walled carbon nanotube dispersion prepared by the method for preparing the multi-walled carbon nanotube dispersion.

[0014] The invention also provides an application of a multi-walled carbon nanotube dispersion in preparing a battery.

[0015] In the preparation method of the present invention, the multi-walled carbon nanotube powder is first subjected to swelling treatment to obtain a relatively loose multi-walled carbon nanotube powder structure, and then bubbles are generated by hydrogen peroxide reaction, and the cavitation effect generated by the bubbles is used to expand and disperse the relatively loose multi-walled carbon nanotube powder structure, and at the same time, the addition of a non-thickening surfactant can significantly improve the treatment effect of expansion and dispersion, so that the multi-walled carbon nanotube powder is easier to disperse by external force, and before the dispersion treatment, the present invention also reduces the degree of free movement between molecules by controlling the concentration of the pre-dispersion liquid and using a thickening surfactant to increase the viscosity of the pre-dispersion liquid, thereby reducing the source of force and the interaction force generated by the dispersion medium distributed to the sites on the carbon nanotubes. Therefore, the preparation method of the present invention can overcome the problem that multi-walled carbon nanotubes are easily broken during the dispersion process, and the multi-walled carbon nanotubes in the obtained dispersion are evenly dispersed and have high stability. Applying it to ion batteries can effectively improve the conductivity and battery capacity of the battery and reduce the cost of ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a SEM image of the multi-walled carbon nanotube dispersant obtained in Example 1; Figure 2 This is a SEM image of the multi-walled carbon nanotube dispersant obtained in Example 7; Figure 3 This is a SEM image of the multi-walled carbon nanotube dispersant obtained in Comparative Example 1; Figure 4 This is a SEM image of the multi-walled carbon nanotube dispersant obtained in Comparative Example 2; Figure 5 This is a SEM image of the multi-walled carbon nanotube dispersant obtained in Comparative Example 5; Figure 6 This is the SEM image of the multi-walled carbon nanotube dispersant obtained in Comparative Example 6. DETAILED DESCRIPTION

[0017] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0019] The method for preparing a multi-walled carbon nanotube dispersion provided by the present invention comprises the following steps: S1, performing swelling treatment on multi-walled carbon nanotube powder to separate and obtain a first intermediate product; S2, mixing the first intermediate product with manganese dioxide and a non-thickening surfactant, then adding hydrogen peroxide to perform expansion treatment, and separating to obtain a second intermediate product; S3, mixing the second intermediate product with a thickening surfactant and a solvent to form a pre-dispersion liquid, and then dispersing the pre-dispersion liquid at least twice to obtain a multi-walled carbon nanotube dispersion liquid, wherein the mass fraction of the second intermediate product in the pre-dispersion liquid is less than 1.5%.

[0020] In step S1, the multi-walled carbon nanotube powder is subjected to swelling treatment to obtain a relatively loose multi-walled carbon nanotube powder structure. The multi-walled carbon nanotube powder is obtained by a fluidized bed method or the like, and the present invention does not limit the source of the multi-walled carbon nanotubes.

[0021] The method for swelling multi-walled carbon nanotube powder in the present invention is not particularly limited. As some specific examples, the swelling treatment method includes but is not limited to using acid to treat multi-walled carbon nanotube powder, lipid solvent to treat multi-walled carbon nanotube powder, etc.

[0022] Preferably, in the present invention, multi-walled carbon nanotube powder is added to acid to perform intercalation swelling on the multi-walled carbon nanotube powder, and after a period of reaction, the powder is washed with water to neutrality and filtered to obtain a first intermediate product.

[0023] The acid is selected from at least one of chlorosulfonic acid, concentrated nitric acid, concentrated sulfuric acid and concentrated hydrochloric acid, more preferably chlorosulfonic acid, the mass ratio of the acid to the multi-walled carbon nanotube powder is 10:1-100:1, the temperature of the swelling treatment is 10°C-60°C, and the time is 15min-8h.

[0024] In step S2, the first intermediate product is mixed with manganese dioxide and a non-thickening surfactant, and then hydrogen peroxide is added. The hydrogen peroxide reacts under the catalysis of manganese dioxide to generate bubbles. The cavitation effect generated by the bubbles causes the swollen carbon nanotubes to expand and disperse, and can prevent the multi-walled carbon nanotubes from breaking. At the same time, the non-thickening surfactant can be fully adsorbed and wrapped on the surface of the multi-walled carbon nanotubes or intercalated in the gaps entangled by the multi-walled carbon nanotubes during the expansion process, and the shrinkage and agglomeration of the multi-walled carbon nanotubes are avoided through steric hindrance and electrostatic repulsion, thereby greatly improving the dispersion of the multi-walled carbon nanotube powder in the solution, so that the multi-walled carbon nanotube powder is evenly suspended in the solution, which significantly improves the expansion treatment effect.

[0025] Optionally, in the step of adding hydrogen peroxide for expansion treatment, the hydrogen peroxide is added in batches, such as dropwise addition. The batch addition may be continuous or intermittent, thereby controlling the rate at which manganese dioxide catalyzes the hydrogen peroxide reaction, thereby controlling the rate at which bubbles are generated, improving the expansion and dispersion effects, and avoiding the breakage of the multi-walled carbon nanotubes.

[0026] Optionally, the mass ratio of the hydrogen peroxide to the manganese dioxide is 10:1-50:1, and the mass ratio of the hydrogen peroxide to the multi-walled carbon nanotube powder is 5:1-50:1.

[0027] Optionally, the expansion treatment is performed at a temperature of 10°C-85°C and for a time of 15min-8h; Optionally, the mass ratio of the non-thickening surfactant to the multi-walled carbon nanotube powder is 1:10-10:10, and the non-thickening surfactant is selected from at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium polystyrene sulfonate, lithium polystyrene sulfonate, sodium lignin sulfonate, alkali lignin, polyvinyl pyrrolidone or sodium dodecyl sulfate.

[0028] After the swelling and expansion treatment of the present invention, the multi-walled carbon nanotube powder is more easily dispersed by external force. In step S3, at least two dispersion treatments are performed, such as two dispersion treatments, three dispersion treatments, etc., to reduce the mechanical force of each dispersion treatment and avoid the breakage of the multi-walled carbon nanotubes.

[0029] In addition, before the dispersion treatment, the present invention first mixes the second intermediate product with a thickening surfactant and a solvent to form a pre-dispersion liquid, wherein the thickening surfactant can increase the viscosity of the pre-dispersion liquid and reduce the degree of free movement between molecules. At the same time, by controlling the concentration of the pre-dispersion liquid, the source of force and the interaction force generated by the dispersion medium can be reduced and distributed to the sites on the dispersed carbon nanotubes, thereby avoiding the breakage of the multi-walled carbon nanotubes.

[0030] Optionally, the solvent is selected from water, the mass ratio of the thickening surfactant to the multi-walled carbon nanotube powder is 2.5:10-15:10, and the thickening surfactant is selected from at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium hexametaphosphate or sodium alginate.

[0031] Optionally, the dispersion treatment method is selected from air flow pulverization, emulsification shearing, colloid milling, ball milling, ultrasonic crushing, high-pressure homogenization or sand milling.

[0032] Optionally, the pre-dispersion liquid is subjected to a primary dispersion treatment and a secondary dispersion treatment in sequence, wherein the primary dispersion treatment is selected from at least one of air flow crushing, emulsification shearing, colloid milling or ball milling, and the secondary dispersion treatment is selected from at least one of ultrasonic crushing, high-pressure homogenization or sand milling.

[0033] Among them, the primary dispersion treatment method is preferably emulsification shearing, the treatment rate of emulsification shearing is 4000rpm-16000rpm, and the treatment time is 15min-360min; the secondary dispersion treatment method is preferably high-pressure homogenization and ultrasonic crushing, the pressure of high-pressure homogenization is 3000psi-16000psi, the power of ultrasonic crushing is 80W-150W, and the time is 15min-1.5h.

[0034] The present invention also provides a multi-walled carbon nanotube dispersion prepared by the method for preparing the multi-walled carbon nanotube dispersion.

[0035] The multi-walled carbon nanotubes in the multi-walled carbon nanotube dispersion prepared by the preparation method of the present invention have good dispersibility and high stability. When applied to ion batteries, they can better wrap around the active material particles in the ion batteries, significantly improving the battery's conductivity and battery capacity.

[0036] The present invention also provides application of the multi-walled carbon nanotube dispersion in batteries.

[0037] After the swelling and expansion treatment of the present invention, the multi-walled carbon nanotube powder is more easily dispersed by external force, and before the dispersion treatment, the present invention also reduces the degree of free movement between molecules by controlling the concentration of the pre-dispersion liquid and using a thickening surfactant to increase the viscosity of the pre-dispersion liquid, thereby reducing the distribution of the interaction force generated by the source of force and the dispersion medium to the sites on the dispersed carbon nanotubes. Therefore, the preparation method of the present invention can overcome the problem that the multi-walled carbon nanotubes are easy to break during the dispersion process, and the multi-walled carbon nanotubes in the obtained dispersion are evenly dispersed and highly stable. Applying it to ion batteries can effectively improve the conductivity and battery capacity of the battery and reduce the cost of ion batteries.

[0038] Hereinafter, the multi-walled carbon nanotube dispersion and its preparation method and application will be further described through the following specific examples.

[0039] Example 1 At 50° C., 6 g of multi-walled carbon nanotube powder was added into 60 g of chlorosulfonic acid for swelling. After 8 hours of swelling, the powder was washed with water until neutral and filtered to obtain a first intermediate product.

[0040] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and then 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the mixture was washed with water until neutral and filtered to obtain a second intermediate product.

[0041] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0042] Example 2 At 50° C., 6 g of multi-walled carbon nanotube powder was added into 60 g of chlorosulfonic acid for swelling. After swelling for 8 hours, the mixture was washed with water until neutral and filtered to obtain a first intermediate product.

[0043] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0044] 3 g of sodium carboxymethyl cellulose and 988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.6%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0045] Example 3 At 50° C., 6 g of multi-walled carbon nanotube powder was swelled in 60 g of chlorosulfonic acid for 8 hours, then washed with water until neutral and filtered to obtain a first intermediate product.

[0046] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0047] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 30 min, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at 80 W for 30 min to obtain a multi-walled carbon nanotube dispersion.

[0048] Example 4 At 50° C., 6 g of multi-walled carbon nanotube powder was swelled in 60 g of chlorosulfonic acid for 8 hours, then washed with water until neutral and filtered to obtain a first intermediate product.

[0049] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0050] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at 10000 psi, 13000 psi, and 16000 psi, respectively, and finally, ultrasonically crushed at 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0051] Example 5 At 50° C., 6 g of multi-walled carbon nanotube powder was swelled in 60 g of chlorosulfonic acid for 8 hours, then washed with water until neutral and filtered to obtain a first intermediate product.

[0052] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0053] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at 80 W for 2 hours to obtain a multi-walled carbon nanotube dispersion.

[0054] Example 6 At 50° C., 6 g of multi-walled carbon nanotube powder was swelled in 60 g of chlorosulfonic acid for 8 hours, then washed with water until neutral and filtered to obtain a first intermediate product.

[0055] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0056] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then sheared in a colloid mill for 1 hour, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively. Finally, ultrasonic crushing was performed at 80 W power for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0057] Example 7 At 50° C., 6 g of multi-walled carbon nanotube powder was swelled in 60 g of chlorosulfonic acid for 8 hours, then washed with water until neutral and filtered to obtain a first intermediate product.

[0058] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0059] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then sand-milled, 50 μm of zirconium oxide was added, and sand-milled at a speed of 1100 rpm for 2 hours. Finally, ultrasonic crushing was performed at a power of 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0060] Example 8 At 50° C., 6 g of multi-walled carbon nanotube powder was swelled in 60 g of chlorosulfonic acid for 8 hours, then washed with water until neutral and filtered to obtain a first intermediate product.

[0061] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0062] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then ultrasonically crushed at 80 W for 60 minutes to obtain a multi-walled carbon nanotube dispersion solution.

[0063] Comparative Example 1 6g of multi-walled carbon nanotube powder, 2g of sodium lignin sulfonate, 1g of polyvinyl pyrrolidone, 3g of sodium carboxymethyl cellulose and 2988ml of deionized water were mixed to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000rpm for 1h, and then high-pressure homogenization was performed at a homogenization pressure of 4000psi, 6000psi, and 3000psi, respectively. Finally, ultrasonic crushing was performed at a power of 100W, and after crushing for 30min, a multi-walled carbon nanotube dispersion solution was obtained.

[0064] Comparative Example 2 At 50° C., 6 g of multi-walled carbon nanotube powder was added into 60 g of chlorosulfonic acid for swelling. After swelling for 8 hours, the mixture was washed with water until neutral and filtered to obtain a first intermediate product.

[0065] The first intermediate product, 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone, 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were mixed to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at a homogenization pressure of 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at a power of 100 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0066] Comparative Example 3 At 50° C., 6 g of multi-walled carbon nanotube powder was added into 60 g of chlorosulfonic acid for swelling. After swelling for 8 hours, the mixture was washed with water until neutral and filtered to obtain a first intermediate product.

[0067] 4 g of manganese dioxide was added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the mixture was washed with water until neutral and filtered to obtain a second intermediate product.

[0068] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone, 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at a homogenization pressure of 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at a power of 100 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0069] Comparative Example 4 At 50° C., 6 g of multi-walled carbon nanotube powder was added into 60 g of chlorosulfonic acid for swelling. After swelling for 8 hours, the mixture was washed with water until neutral and filtered to obtain a first intermediate product.

[0070] 3 g of sodium carboxymethyl cellulose and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0071] 3 g of sodium lignin sulfonate and 2988 ml of deionized water were added to the second intermediate product, and emulsification shearing was performed at 7000 rpm for 1 hour. High-pressure homogenization was then performed with homogenization pressures of 4000 psi, 6000 psi, and 3000 psi respectively. Finally, ultrasonic crushing was performed at 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0072] Comparative Example 5 At 50° C., 6 g of multi-walled carbon nanotube powder was added into 60 g of chlorosulfonic acid for swelling. After swelling for 8 hours, the mixture was washed with water until neutral and filtered to obtain a first intermediate product.

[0073] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0074] 3 g of sodium lignin sulfonate and 2988 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0075] Comparative Example 6 At 50°C, 6 g of multi-walled carbon nanotube powder, 60 g of chlorosulfonic acid, 4 g of manganese dioxide and 40 g of hydrogen peroxide were swollen and expanded, 2 g of sodium lignin sulfonate and 1 g of polyvinyl pyrrolidone were added for 8 hours, then washed with water to neutrality and filtered to obtain a first intermediate product.

[0076] 3 g of sodium carboxymethyl cellulose and 2988 ml of deionized water were added to the first intermediate product to obtain a pre-dispersion solution with a concentration of 0.2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0077] Comparative Example 7 At 50° C., 6 g of multi-walled carbon nanotube powder was added into 60 g of chlorosulfonic acid for swelling. After swelling for 8 hours, the mixture was washed with water until neutral and filtered to obtain a first intermediate product.

[0078] 2 g of sodium lignin sulfonate, 1 g of polyvinyl pyrrolidone and 4 g of manganese dioxide were added to the first intermediate product, and 40 g of hydrogen peroxide was slowly added dropwise. After reacting at 50° C. for 8 hours, the product was washed with water until neutral and filtered to obtain a second intermediate product.

[0079] 3 g of sodium carboxymethyl cellulose and 288 ml of deionized water were added to the second intermediate product to obtain a pre-dispersion solution with a concentration of 2%. The pre-dispersion solution was then emulsified and sheared at 7000 rpm for 1 hour, and then high-pressure homogenized at 4000 psi, 6000 psi, and 3000 psi, respectively, and finally, ultrasonically crushed at 80 W for 30 minutes to obtain a multi-walled carbon nanotube dispersion.

[0080] The multi-walled carbon nanotube dispersions obtained in Examples 1 to 8 and Comparative Examples 1 to 7 were subjected to particle size analysis and viscosity characterization. The results are shown in Table 1.

[0081] Steps for particle size analysis: add the multi-walled carbon nanotube dispersion dropwise into a laser particle size analyzer beaker filled with deionized water until the transmittance is between 5% and 10%; Viscosity measurement steps: Weigh 2 ml of multi-walled carbon nanotube dispersion and place it on the sample stage of the high and low temperature viscometer, set the temperature to 25°C, adjust the gap, and -1 The viscosity is measured at a shear rate of 1.

[0082] Table 1 As can be seen from Table 1, by adopting the preparation method of the present invention, the multi-walled carbon nanotubes in the obtained dispersion are evenly dispersed and highly stable. Meanwhile, the dispersion prepared by the present invention has a relatively low viscosity and excellent processability.

[0083] In addition, the multi-walled carbon nanotube dispersions obtained in some embodiments and comparative examples were tested by scanning electron microscopy (SEM test). The test steps were as follows: a drop of multi-walled carbon nanotube dispersion was taken and diluted 100 times, ultrasonicated for 10 minutes, and the ultrasonicated sample was dropped on the surface of the silicon wafer for observation. The results were as follows: Figures 1 to 6 shown.

[0084] from Figure 1 and Figure 2 It can be seen that the gaps between the multi-walled carbon nanotubes are clear, there is less agglomeration, and they mainly present relatively independent individuals, indicating that they are evenly dispersed in the dispersion. In addition, the multi-walled carbon nanotubes in the dispersion are relatively long and have less breakage.

[0085] Comparative Example 1 uses conventional dispersion means to disperse multi-walled carbon nanotube powder without swelling and expansion treatment, and the D50 particle size of the dispersion is larger than the D50 particle size in all the examples. Figure 3 It can be seen that since the dispersion has not undergone the swelling and expansion process, there are still many large-sized multi-walled carbon nanotube powders in the dispersion, and most of the multi-walled carbon nanotubes are still tightly entangled after dispersion, and the dispersibility is poor. Therefore, the absorbance of the dispersion is poor, the optical density is lower than that of the embodiment, and the optical density after centrifugation is also significantly different from that before centrifugation, and the stability is poor.

[0086] Compared with all the examples, Comparative Example 2 did not undergo the expansion process. Compared with Comparative Example 1, the particle size D50 of the dispersion was smaller than that of Comparative Example 1, indicating that the dispersibility of the multi-walled carbon nanotube powder was relatively improved after swelling. Figure 4 It can be seen that the multi-walled carbon nanotube powder in the dispersion begins to have a tendency to disentangle and loosen, but compared with the embodiments, the particle size D50 of the dispersion is larger than that of all the embodiments.

[0087] In Comparative Example 3, no non-thickening surfactant was added during the expansion process, and the particle size D50 in the dispersion was larger than that in all the embodiments, indicating that the introduction of the non-thickening surfactant during the expansion process can effectively avoid the agglomeration of multi-walled carbon nanotubes during the filtration process.

[0088] Comparative Example 4 introduced a thickening dispersant during the expansion process, so it has a higher viscosity than the dispersion of the embodiment. The particle size analysis shows that the particle size in Comparative Example 4 is larger, which leads to a large number of agglomerates and a large particle size in the dispersion, thereby affecting its dispersibility. This shows that a high viscosity environment will greatly affect the dispersion efficiency and increase the dispersion resistance.

[0089] Comparative Example 5 uses a non-thickening surfactant in both the expansion and subsequent dispersion processes, and has a lower viscosity. As shown in Table 1, the particle size D50 of the dispersion is smaller than that of Example 1 and the comparative example, with fewer agglomerate structures and smaller particle sizes. Figure 5 It can be seen that there are almost no agglomerates and undispersed multi-walled carbon nanotube powders in the slurry, and the dispersibility is excellent. However, due to the low viscosity of the system, which is almost similar to that of the solvent, the free movement of the particles in the solvent environment reaches the maximum, and the interaction between the force and the dispersion medium is more easily distributed to the sites on the dispersed medium. Therefore, the shear force, cavitation effect and impact effect are stronger in a high viscosity environment, making the originally rigid multi-walled carbon nanotube powder easier to break during the dispersion process. Therefore, the length of the multi-walled carbon nanotubes in the dispersion is shorter than that in the embodiment.

[0090] Comparative Example 6 was subjected to both swelling and expansion processes. As shown in Table 1, the particle size D50 of the dispersion was larger than that of all the examples. Figure 6 It can be seen that the carbon nanotube powders in the dispersion are completely dispersed, and there is no array structure in the dispersion. However, the dispersed multi-walled carbon nanotubes are severely entangled and broken. Most of the multi-walled carbon nanotubes are tightly intertwined and distributed in blocks at various positions. This is because the strong acidity during the swelling and expansion process inhibits the ionization ability of the non-thickening surfactant in the solution, thereby weakening the ability of the non-thickening surfactant molecules to adsorb and wrap on the surface of the multi-walled carbon nanotubes, thereby generating steric hindrance and electrostatic repulsion to prevent their agglomeration. At the same time, polymer surfactants such as PVP are easily denatured and inactivated under strong acid conditions, so their ability to provide adsorption and steric hindrance is greatly reduced, so that the multi-walled carbon nanotubes still shrink after expansion, thereby causing entanglement-type agglomeration.

[0091] The concentration of the second intermediate product in Comparative Example 7 is greatly increased compared with that in Example. It can be seen from Table 1 that the particle size of the dispersion is similar to that in Comparative Example 4, and both are much larger than the particle size D50 in Example. It can be seen that there are still many large-sized agglomerate structures in the dispersion, and the dispersibility is poor. This is because the increase in the number of particles in the system also affects the interaction between the source of force and the dispersion medium.

[0092] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0093] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a multi-walled carbon nanotube dispersion, characterized in that: The steps include: Swelling the multi-walled carbon nanotube powder to obtain a first intermediate product; The first intermediate product is mixed with manganese dioxide and a non-thickening surfactant, and then hydrogen peroxide is added to perform expansion treatment, and a second intermediate product is obtained by separation; The second intermediate product is mixed with a thickening surfactant and a solvent to form a pre-dispersion liquid, and then the pre-dispersion liquid is dispersed at least twice to obtain a multi-walled carbon nanotube dispersion liquid, wherein the mass fraction of the second intermediate product in the pre-dispersion liquid is less than 1.5%.

2. The method for preparing a multi-walled carbon nanotube dispersion according to claim 1, characterized in that: In the step of subjecting the multi-walled carbon nanotube powder to swelling treatment, the multi-walled carbon nanotube powder is mixed with an acid to perform swelling treatment.

3. The method for preparing a multi-walled carbon nanotube dispersion according to claim 2, characterized in that: The step of mixing the multi-walled carbon nanotube powder with an acid for swelling treatment satisfies at least one of the following conditions: (1) The acid is at least one selected from chlorosulfonic acid, concentrated nitric acid, concentrated sulfuric acid, and concentrated hydrochloric acid; (2) The mass ratio of the acid to the multi-walled carbon nanotube powder is 10:1-100:1; (3) The swelling treatment is carried out at a temperature of 10°C to 60°C and for a time of 15 min to 8 h.

4. The method for preparing a multi-walled carbon nanotube dispersion according to claim 1, characterized in that: In the step of adding hydrogen peroxide for expansion treatment, the hydrogen peroxide is added in batches.

5. The method for preparing a multi-walled carbon nanotube dispersion according to claim 1 or claim 4, characterized in that: The expansion step also satisfies at least one of the following conditions: (1) The mass ratio of the hydrogen peroxide to the manganese dioxide is 10:1-50:1; (2) The mass ratio of the hydrogen peroxide to the multi-walled carbon nanotube powder is 5:1-50:1; (3) The expansion treatment is carried out at a temperature of 10°C to 85°C and for a time of 15 minutes to 8 hours; (4) The mass ratio of the non-thickening surfactant to the multi-walled carbon nanotube powder is 1:10-10:10; (5) The non-thickening surfactant is selected from at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium polystyrene sulfonate, lithium polystyrene sulfonate, sodium lignin sulfonate, alkali lignin, polyvinyl pyrrolidone or sodium dodecyl sulfate.

6. The method for preparing a multi-walled carbon nanotube dispersion according to claim 1, characterized in that: The pre-dispersion liquid also satisfies at least one of the following conditions: (1) The mass ratio of the thickening surfactant to the multi-walled carbon nanotube powder is 2.5:10-15:10; (2) The thickening surfactant is at least one selected from sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium hexametaphosphate or sodium alginate; (3) The solvent is selected from water.

7. The method for preparing a multi-walled carbon nanotube dispersion according to claim 1, characterized in that: The dispersion treatment method is selected from air flow pulverization, emulsification shearing, colloid milling, ball milling, ultrasonic crushing, high-pressure homogenization or sand milling.

8. The method for preparing a multi-walled carbon nanotube dispersion according to claim 1 or claim 7, characterized in that: The pre-dispersion liquid is sequentially subjected to a primary dispersion treatment and a secondary dispersion treatment, wherein the primary dispersion treatment is selected from at least one of air flow crushing, emulsification shearing, colloid milling or ball milling, and the secondary dispersion treatment is selected from at least one of ultrasonic crushing, high-pressure homogenization or sand milling. 9 . A multi-walled carbon nanotube dispersion prepared by the method for preparing a multi-walled carbon nanotube dispersion according to any one of claims 1 to 8 .

10. Use of the multi-walled carbon nanotube dispersion according to claim 9 in preparing a battery.

Citation Information

Patent Citations

  • Simple method for dispersing carbon nano-tube

    CN101485962A

  • Method for treating heavy metal ion wastewater with modified shell powder

    CN105561912A

  • Solid carbon nanotube dispersion method

    CN115465855A

  • High-stability low-viscosity carbon nanotube conductive paste and preparation method thereof

    CN115763798A

  • High-dispersion and high-length-diameter-ratio carbon nano tube, high-solid-content conductive slurry and preparation method of high-dispersion and high-length-diameter-ratio carbon nano tube

    CN117566727A