Production method for producing industrial salt from chlor-alkali by ionic membrane method
The ion membrane method of chlor-alkali production of industrial salts has been solved, and the problem of impurity wrapping or adsorption in brine evaporation has been achieved, high purity preparation of industrial salts has been achieved, and purification costs and exhaust gas emissions have been reduced, which has significantly improved the purity of salts.
Patent Information
- Application Number
- CN202411569985.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing brine evaporation method in the preparation process of industrial salts causes impurities to be wrapped or adsorbed during the salt crystallization process, increasing the impurities content in industrial salts, and the content of impurities such as calcium ions, magnesium ions and sulfate exceeds the national standards. .
The method of producing industrial salt by chlor-alkali by ion membrane method is used to filtration and pH adjustment after brine is extracted, lime milk, sodium carbonate and precipitant are added, combined with boiler flue gas to remove impurities, and then evaporate and salt drying, and finally pass Wash, filter and dry to give industrial salt.
It significantly reduces the calcium ions, magnesium ions and sulfate content in industrial salts, improves the purity of the salt, and uses cheap impurity removal materials, reduces industrial waste gas emissions, and is environmentally friendly.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of industrial salt preparation methods, in particular to a method for producing industrial salt using chlorine-alkali ion membrane method. Background Art
[0002] Industrial salt is one of the most basic raw materials of the chemical industry. Its main components include sodium chloride and sodium nitrite, and it is known as the "mother of the chemical industry." Hydrochloric acid, caustic soda, soda ash, ammonium chloride, chlorine, and other major products of the basic chemical industry are mainly produced using industrial salt as raw materials.
[0003] Industrial salt has many applications. It is used as a desulfurizer in the steel smelting process, used for road deicing in winter to prevent road icing and improve driving safety, and used in the preparation of drilling fluid in the oil drilling process to prevent well wall collapse. In addition, although industrial salt is not directly used in food processing, it may be used in some food industries such as pickling and fermentation.
[0004] The existing industrial salt is generally prepared by evaporating and crystallizing brine (groundwater or seawater containing a high concentration of NaCl) through the brine evaporation method. When preparing industrial salt by the existing brine evaporation method, the water gradually evaporates during the brine evaporation process, the salt concentration continues to increase, and the impurities will be concentrated accordingly. The solubility of impurities and the solubility of salt change with temperature and concentration differently, which may cause the impurities to be wrapped or adsorbed on the surface of the salt crystals during the salt crystallization process, thereby increasing the impurity content in the industrial salt.
[0005] Therefore, it is necessary to provide a new ion membrane method for producing industrial salt by chlor-alkali to solve the above technical problems. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for producing industrial salt by using chlor-alkali through an ion membrane process.
[0007] The method for producing industrial salt by chlor-alkali process using an ion membrane method provided by the present invention comprises the following steps: S1: extracting brine; S2: Filter the brine and adjust the pH of the brine to 8.5-9.5; S3: adding lime milk, sodium carbonate and a precipitating agent to the brine, wherein the amount of lime milk added is 0.1-0.2 g / L, the amount of sodium carbonate added is 0.02-0.05 g / L, and the amount of the precipitating agent added is 0.001-0.003 g / L, standing for 2-3 hours, removing the filter residue, and obtaining a primary filtrate; S4: introducing boiler flue gas into the primary filtrate. When the pH of the primary filtrate reaches 6.5-7.5, stop introducing boiler flue gas and remove the filter residue to obtain a secondary filtrate. S5: Pump the secondary filtrate to the evaporation tank, add the waste from the ammonia-soda process, mix well, and let stand for 5-8 hours; S6: evaporating and drying the secondary filtrate of the waste material of the ammonia-soda process to obtain primary salt; S7: Wash, filter and dry the initial salt in step S6 to obtain industrial salt.
[0008] Preferably, when boiler flue gas is added to the primary filtrate, the temperature of the boiler flue gas is 15-25°C.
[0009] Preferably, the precipitation aid is one or more of polyacrylamide, sodium polyacrylate and polydimethyldiallylammonium chloride.
[0010] Preferably, in step S5, the depth of the brine in the evaporation pond is 6-10 cm in spring and autumn, 8-12 cm in summer, and 4-8 cm in winter.
[0011] Preferably, in the step S2, when filtering the brine, coarse filtration is first performed and then fine filtration is performed.
[0012] Preferably, the brine passes through a first filter tank and a second filter tank respectively during coarse filtration, wherein the first filter tank contains anthracite, quartz sand and pebbles, wherein the bottom layer is pebbles with a particle size of 2.5-5.5 mm, the middle layer is quartz sand with a particle size of 0.6-1.2 mm, and the top layer is anthracite with a particle size of 0.8-1.8 mm.
[0013] Preferably, the second filter tank contains quartz sand, manganese sand and magnetite, wherein the bottom layer is magnetite with a particle size of 1.0-2.0 mm, the middle layer is manganese sand with a particle size of 0.4-1.0 mm, and the top layer is quartz sand with a particle size of 0.6-1.2 mm.
[0014] Preferably, the filtration rate of the first filter tank is 20-30m³ / (h·m²), and the filtration rate of the second filter tank is 5-10m³ / (h·m²).
[0015] Preferably, the fine filtration includes microfiltration and ultrafiltration, the pore size of the microfiltration membrane is 0.3-0.5 μm, the operating pressure during the microfiltration treatment is 50-80 kPa, the pore size of the ultrafiltration membrane is 0.05-0.1 μm, and the operating pressure during the ultrafiltration treatment is 100-300 kPa.
[0016] Preferably, the brine is extracted from underground or a salt lake.
[0017] Compared with the related art, the production method of industrial salt produced by chlor-alkali ion membrane method provided by the present invention has the following beneficial effects: The calcium ion content, magnesium ion content and sulfate content in the industrial salt prepared by the method provided by the present invention are all lower than the calcium ion content, magnesium ion content and sulfate content specified in the national standards, which indicates that the calcium ion content, magnesium ion content and sulfate content of impurities in the industrial salt prepared by the method of the present invention are low, so that the purity of the prepared industrial salt is improved.
[0018] The present invention uses lime milk and boiler flue gas for impurity removal. The impurity removal materials are cheap and easy to obtain, which reduces the cost of purifying brine to a certain extent, and reduces the emission of industrial waste gas, which is more environmentally friendly. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with the embodiments.
[0020] In the specific implementation process, Embodiment 1
[0021] The production method of industrial salt produced by chlor-alkali process using ion membrane method comprises the following steps: S1: Extraction of brine, brine is extracted from underground or salt lakes; S2: Filter the brine and adjust the pH of the brine to 8.5-9.5; S3: adding lime milk, sodium carbonate and a precipitating agent to the brine, wherein the amount of lime milk added is 0.15 g / L, the amount of sodium carbonate added is 0.035 g / L, the amount of the precipitating agent added is 0.002 g / L, and the precipitating agent is one or more of polyacrylamide, sodium polyacrylate and polydimethyldiallylammonium chloride, standing for 2-3 hours, removing the filter residue, and obtaining a primary filtrate; S4: introducing boiler flue gas into the primary filtrate, the temperature of the boiler flue gas being 15-25°C. When the pH of the primary filtrate reaches 6.5-7.5, stop introducing the boiler flue gas, remove the filter residue, and obtain the secondary filtrate; S5: Pump the secondary filtrate to the evaporation pond. The depth of the brine in the evaporation pond is 6-10 cm in spring and autumn, 8-12 cm in summer, and 4-8 cm in winter. Add the waste from the ammonia-soda process, mix well, and let it stand for 5-8 hours. S6: evaporating and drying the secondary filtrate of the waste material of the ammonia-soda process to obtain primary salt; S7: Wash, filter and dry the initial salt in step S6 to obtain industrial salt.
[0022] In the step S2, when filtering the brine, it is first coarsely filtered and then finely filtered. When the brine is coarsely filtered, it passes through the first filter tank and the second filter tank respectively. The first filter tank contains anthracite, quartz sand and pebbles, wherein the bottom layer is pebbles with a particle size of 2.5-5.5 mm, the middle layer is quartz sand with a particle size of 0.6-1.2 mm, and the top layer is anthracite with a particle size of 0.8-1.8 mm. The second filter tank contains quartz sand, manganese sand and magnetite, wherein the bottom layer is magnetite with a particle size of 1.0-2.0 mm. The middle layer is manganese sand with a particle size of 0.4-1.0 mm, the top layer is quartz sand with a particle size of 0.6-1.2 mm, the filtration rate of the first filter tank is 20-30 m³ / (h·m²), the filtration rate of the second filter tank is 5-10 m³ / (h·m²), the fine filtration includes microfiltration and ultrafiltration, the pore size of the microfiltration membrane is 0.3-0.5 μm, the operating pressure during the microfiltration treatment is 50-80 kPa, the pore size of the ultrafiltration membrane is 0.05-0.1 μm, and the operating pressure during the ultrafiltration treatment is 100-300 kPa. Embodiment 2
[0023] The production method of industrial salt produced by chlor-alkali process using ion membrane method comprises the following steps: S1: Extraction of brine, brine is extracted from underground or salt lakes; S2: Filter the brine and adjust the pH of the brine to 8.5-9.5; S3: adding lime milk, sodium carbonate and a precipitating agent to the brine, wherein the amount of lime milk added is 0.1 g / L, the amount of sodium carbonate added is 0.02 g / L, the amount of the precipitating agent added is 0.001 g / L, and the precipitating agent is one or more of polyacrylamide, sodium polyacrylate and polydimethyldiallylammonium chloride, standing for 2-3 hours, removing the filter residue, and obtaining a primary filtrate; S4: introducing boiler flue gas into the primary filtrate, the temperature of the boiler flue gas being 15-25°C. When the pH of the primary filtrate reaches 6.5-7.5, stop introducing the boiler flue gas, remove the filter residue, and obtain the secondary filtrate; S5: Pump the secondary filtrate to the evaporation pond. The depth of the brine in the evaporation pond is 6-10 cm in spring and autumn, 8-12 cm in summer, and 4-8 cm in winter. Add the waste from the ammonia-soda process, mix well, and let it stand for 5-8 hours. S6: evaporating and drying the secondary filtrate of the waste material of the ammonia-soda process to obtain primary salt; S7: Wash, filter and dry the initial salt in step S6 to obtain industrial salt.
[0024] In the step S2, when filtering the brine, it is first coarsely filtered and then finely filtered. When the brine is coarsely filtered, it passes through the first filter tank and the second filter tank respectively. The first filter tank contains anthracite, quartz sand and pebbles, wherein the bottom layer is pebbles with a particle size of 2.5-5.5 mm, the middle layer is quartz sand with a particle size of 0.6-1.2 mm, and the top layer is anthracite with a particle size of 0.8-1.8 mm. The second filter tank contains quartz sand, manganese sand and magnetite, wherein the bottom layer is magnetite with a particle size of 1.0-2.0 mm. The middle layer is manganese sand with a particle size of 0.4-1.0 mm, the top layer is quartz sand with a particle size of 0.6-1.2 mm, the filtration rate of the first filter tank is 20-30 m³ / (h·m²), the filtration rate of the second filter tank is 5-10 m³ / (h·m²), the fine filtration includes microfiltration and ultrafiltration, the pore size of the microfiltration membrane is 0.3-0.5 μm, the operating pressure during the microfiltration treatment is 50-80 kPa, the pore size of the ultrafiltration membrane is 0.05-0.1 μm, and the operating pressure during the ultrafiltration treatment is 100-300 kPa. Embodiment 3
[0025] The production method of industrial salt produced by chlor-alkali process using ion membrane method comprises the following steps: S1: Extraction of brine, brine is extracted from underground or salt lakes; S2: Filter the brine and adjust the pH of the brine to 8.5-9.5; S3: adding lime milk, sodium carbonate and a precipitating agent to the brine, wherein the amount of lime milk added is 0.2 g / L, the amount of sodium carbonate added is 0.05 g / L, the amount of the precipitating agent added is 0.003 g / L, and the precipitating agent is one or more of polyacrylamide, sodium polyacrylate and polydimethyldiallylammonium chloride, standing for 2-3 hours, removing the filter residue, and obtaining a primary filtrate; S4: introducing boiler flue gas into the primary filtrate, the temperature of the boiler flue gas being 15-25°C. When the pH of the primary filtrate reaches 6.5-7.5, stop introducing the boiler flue gas, remove the filter residue, and obtain the secondary filtrate; S5: Pump the secondary filtrate to the evaporation pond. The depth of the brine in the evaporation pond is 6-10 cm in spring and autumn, 8-12 cm in summer, and 4-8 cm in winter. Add the waste from the ammonia-soda process, mix well, and let it stand for 5-8 hours. S6: evaporating and drying the secondary filtrate of the waste material of the ammonia-soda process to obtain primary salt; S7: Wash, filter and dry the initial salt in step S6 to obtain industrial salt.
[0026] In the step S2, when filtering the brine, it is first coarsely filtered and then finely filtered. When the brine is coarsely filtered, it passes through the first filter tank and the second filter tank respectively. The first filter tank contains anthracite, quartz sand and pebbles, wherein the bottom layer is pebbles with a particle size of 2.5-5.5 mm, the middle layer is quartz sand with a particle size of 0.6-1.2 mm, and the top layer is anthracite with a particle size of 0.8-1.8 mm. The second filter tank contains quartz sand, manganese sand and magnetite, wherein the bottom layer is magnetite with a particle size of 1.0-2.0 mm. The middle layer is manganese sand with a particle size of 0.4-1.0 mm, the top layer is quartz sand with a particle size of 0.6-1.2 mm, the filtration rate of the first filter tank is 20-30 m³ / (h·m²), the filtration rate of the second filter tank is 5-10 m³ / (h·m²), the fine filtration includes microfiltration and ultrafiltration, the pore size of the microfiltration membrane is 0.3-0.5 μm, the operating pressure during the microfiltration treatment is 50-80 kPa, the pore size of the ultrafiltration membrane is 0.05-0.1 μm, and the operating pressure during the ultrafiltration treatment is 100-300 kPa. Comparative Example 1
[0027] The production method of industrial salt produced by chlor-alkali process using ion membrane method comprises the following steps: S1: Extraction of brine, brine is extracted from underground or salt lakes; S2: Filter the brine and adjust the pH of the brine to 8.5-9.5; S3: adding lime milk, sodium carbonate and a precipitating agent to the brine, wherein the amount of lime milk added is 0.15 g / L, the amount of sodium carbonate added is 0.035 g / L, the amount of the precipitating agent added is 0.002 g / L, and the precipitating agent is one or more of polyacrylamide, sodium polyacrylate and polydimethyldiallylammonium chloride, standing for 2-3 hours, removing the filter residue, and obtaining a primary filtrate; S4: Pump the primary filtrate to the evaporation pond. The depth of the brine in the evaporation pond is 6-10 cm in spring and autumn, 8-12 cm in summer, and 4-8 cm in winter. Add the waste from the ammonia-soda process, mix well, and let it stand for 5-8 hours. S5: evaporating and drying the primary filtrate of the waste material of the ammonia-soda process to obtain primary salt; S6: Wash, filter and dry the initial salt in step S5 to obtain industrial salt.
[0028] In the step S2, when filtering the brine, it is first coarsely filtered and then finely filtered. When the brine is coarsely filtered, it passes through the first filter tank and the second filter tank respectively. The first filter tank contains anthracite, quartz sand and pebbles, wherein the bottom layer is pebbles with a particle size of 2.5-5.5 mm, the middle layer is quartz sand with a particle size of 0.6-1.2 mm, and the top layer is anthracite with a particle size of 0.8-1.8 mm. The second filter tank contains quartz sand, manganese sand and magnetite, wherein the bottom layer is magnetite with a particle size of 1.0-2.0 mm. The middle layer is manganese sand with a particle size of 0.4-1.0 mm, the top layer is quartz sand with a particle size of 0.6-1.2 mm, the filtration rate of the first filter tank is 20-30 m³ / (h·m²), the filtration rate of the second filter tank is 5-10 m³ / (h·m²), the fine filtration includes microfiltration and ultrafiltration, the pore size of the microfiltration membrane is 0.3-0.5 μm, the operating pressure during the microfiltration treatment is 50-80 kPa, the pore size of the ultrafiltration membrane is 0.05-0.1 μm, and the operating pressure during the ultrafiltration treatment is 100-300 kPa. Comparative Example 2
[0029] The production method of industrial salt produced by chlor-alkali process using ion membrane method comprises the following steps: S1: Extraction of brine, brine is extracted from underground or salt lakes; S2: filtering the brine; S3: Pump the filtered brine to the evaporation pond. The depth of the brine in the evaporation pond is 6-10cm in spring and autumn, 8-12cm in summer, and 4-8cm in winter. Add the waste from the ammonia-soda process, mix well, and let it stand for 5-8h. S4: evaporating and drying the solution to which the waste material of the ammonia-soda process is added to obtain primary salt; S5: Wash, filter and dry the initial salt in step S4 to obtain industrial salt.
[0030] In the step S2, when filtering the brine, it is first coarsely filtered and then finely filtered. When the brine is coarsely filtered, it passes through the first filter tank and the second filter tank respectively. The first filter tank contains anthracite, quartz sand and pebbles, wherein the bottom layer is pebbles with a particle size of 2.5-5.5 mm, the middle layer is quartz sand with a particle size of 0.6-1.2 mm, and the top layer is anthracite with a particle size of 0.8-1.8 mm. The second filter tank contains quartz sand, manganese sand and magnetite, wherein the bottom layer is magnetite with a particle size of 1.0-2.0 mm. The middle layer is manganese sand with a particle size of 0.4-1.0 mm, the top layer is quartz sand with a particle size of 0.6-1.2 mm, the filtration rate of the first filter tank is 20-30 m³ / (h·m²), the filtration rate of the second filter tank is 5-10 m³ / (h·m²), the fine filtration includes microfiltration and ultrafiltration, the pore size of the microfiltration membrane is 0.3-0.5 μm, the operating pressure during the microfiltration treatment is 50-80 kPa, the pore size of the ultrafiltration membrane is 0.05-0.1 μm, and the operating pressure during the ultrafiltration treatment is 100-300 kPa. Experimental Group
[0031] The impurity components of the industrial salts prepared in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 were measured, and the results are shown in the following table:
[0032] Analysis of the data in the above table shows that the calcium ion content, magnesium ion content and sulfate content in the industrial salt prepared by the methods provided in Examples 1, 2 and 3 of the present invention are lower than those in Comparative Examples 1 and 2, which indicates that the impurity content in the industrial salt prepared by the method of the present invention is low, and the present invention uses lime milk and boiler flue gas for impurity removal, and the impurity removal materials are cheap and easy to obtain. To a certain extent, the cost of purifying brine is reduced, while reducing the emission of industrial waste gas, which is more environmentally friendly.
[0033] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for producing industrial salt by using chlorine-alkali ion membrane method, characterized in that: The following steps are involved: S1: extracting brine; S2: Filter the brine and adjust the pH of the brine to 8.5-9.5; S3: adding lime milk, sodium carbonate and a precipitating agent to the brine, wherein the amount of lime milk added is 0.1-0.2 g / L, the amount of sodium carbonate added is 0.02-0.05 g / L, and the amount of the precipitating agent added is 0.001-0.003 g / L, standing for 2-3 hours, removing the filter residue, and obtaining a primary filtrate; S4: introducing boiler flue gas into the primary filtrate. When the pH of the primary filtrate reaches 6.5-7.5, stop introducing boiler flue gas and remove the filter residue to obtain a secondary filtrate. S5: Pump the secondary filtrate to the evaporation tank, add the waste from the ammonia-soda process, mix well, and let stand for 5-8 hours; S6: evaporating and drying the secondary filtrate of the waste material of the ammonia-soda process to obtain primary salt; S7: Wash, filter and dry the initial salt in step S6 to obtain industrial salt.
2. The method for producing industrial salt by using chlor-alkali ion membrane method according to claim 1, characterized in that: When boiler flue gas is added to the primary filtrate, the temperature of the boiler flue gas is 15-25°C.
3. The method for producing industrial salt by using chlor-alkali ion membrane method according to claim 1, characterized in that: The precipitation aid is one or more of polyacrylamide, sodium polyacrylate and polydimethyldiallylammonium chloride.
4. The method for producing industrial salt by using chlor-alkali ion membrane method according to claim 1, characterized in that: In the step S5, the depth of the brine in the evaporation pond is 6-10 cm in spring and autumn, 8-12 cm in summer, and 4-8 cm in winter.
5. The method for producing industrial salt by using chlor-alkali ion membrane method according to claim 1, characterized in that: In the step S2, when filtering the brine, coarse filtration is first performed and then fine filtration is performed.
6. The method for producing industrial salt by using chlor-alkali through ion membrane method according to claim 5, characterized in that: When the brine is coarsely filtered, it passes through the first filter tank and the second filter tank respectively. The first filter tank contains anthracite, quartz sand and pebbles, wherein the bottom layer is pebbles with a particle size of 2.5-5.5 mm, the middle layer is quartz sand with a particle size of 0.6-1.2 mm, and the top layer is anthracite with a particle size of 0.8-1.8 mm.
7. The method for producing industrial salt by using chlor-alkali ion membrane method according to claim 6, characterized in that: The second filter tank contains quartz sand, manganese sand and magnetite, wherein the bottom layer is magnetite with a particle size of 1.0-2.0 mm, the middle layer is manganese sand with a particle size of 0.4-1.0 mm, and the top layer is quartz sand with a particle size of 0.6-1.2 mm.
8. The method for producing industrial salt by using chlor-alkali ion membrane method according to claim 6, characterized in that: The filtration rate of the first filter tank is 20-30m³ / (h·m²), and the filtration rate of the second filter tank is 5-10m³ / (h·m²).
9. The method for producing industrial salt by using chlor-alkali through ion membrane method according to claim 5, characterized in that: The fine filtration includes microfiltration and ultrafiltration. The pore size of the microfiltration membrane is 0.3-0.5 μm, and the operating pressure during the microfiltration treatment is 50-80 kPa. The pore size of the ultrafiltration membrane is 0.05-0.1 μm, and the operating pressure during the ultrafiltration treatment is 100-300 kPa.
10. The method for producing industrial salt by using chlor-alkali through ion membrane method according to claim 1, characterized in that: The brine is extracted from underground or salt lakes.
Citation Information
Patent Citations
Method for preparing dedicated Industrial salt for producing chlorine alkali through ion membrane method
CN101049949A
Technological process for purifying bittern
CN101289200A
Purification method of lime-flue gas brine
CN106986356A
Lime flue gas brine purification method
CN109574041A
Novel preparation process for co-producing refined salt and anhydrous nitrate from refined liquid salt applied to alkali production
CN111087006A
Cited By
Preparation method of special industrial salt for chlor-alkali production by ionic membrane method
CN119490205A
A method for preparing industrial salt for chlor-alkali production by ion membrane method
CN119490205B