Calcium carbonate nanofluid as well as preparation method and application thereof

Stable calcium carbonate nanofluids were prepared by neutralizing hydrolyzed polymaleic anhydride with alkaline solution after neutralization of hydrolyzed polymaleic anhydride and alkaline solution in low permeability reservoirs, and the poor stability of nanofluids was solved. The problem of this paper improves the recovery rate and emulsification performance of the reservoir.

CN119059545AActive Publication Date: 2024-12-03CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411171414.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing nanofluids have poor stability and high cost in low permeability reservoirs, making it difficult to effectively improve reservoir recovery.

Method used

By mixing hydrolyzed polymaleic anhydride with alkali solution and chelating precipitation reaction with soluble calcium salt and carbonate solution, calcium carbonate nanofluid with excellent stability is prepared to improve the stability and emulsification performance of the nanofluid.

Benefits of technology

The prepared calcium carbonate nanofluid still had 46% of the unprecipitated after 10 days of standing, which had good performance and emulsification properties to reduce interfacial tension, significantly improving the recovery rate of the reservoir.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059545A_ABST
    Figure CN119059545A_ABST
Patent Text Reader

Abstract

The invention provides a calcium carbonate nanofluid as well as a preparation method and application thereof, and belongs to the technical field of functional materials. According to the invention, hydrolytic polymaleic anhydride, water and alkali liquor are mixed and then subjected to neutralization reaction, so that carboxyl in hydrolytic polymaleic anhydride is changed into carboxylate radical, which is convenient for subsequent chelation with calcium ions; a soluble calcium salt solution and a soluble carbonate solution are dropwise added into a mixed solution for a chelating precipitation reaction, in the reaction process, on one hand, calcium ions are chelated with hydrolytic polymaleic anhydride, on the other hand, the calcium ions react with carbonate to form calcium carbonate, then the calcium carbonate nanofluid is formed, and the calcium carbonate nanofluid is obtained through the synchronous chelating precipitation reaction. According to the invention, the stability of the nanofluid is improved, and the nanofluid has good interfacial tension reduction performance and emulsibility, and has excellent oil reservoir recovery efficiency when used as an oil-displacing agent for oilfield exploitation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and specifically relates to a calcium carbonate nanofluid and a preparation method and application thereof. Background Art

[0002] Low permeability reservoirs have abundant reserves worldwide and have significant production potential, so they have gradually become an important focus of research and development in the oil and gas industry. Nanofluid displacement technology is widely used to improve the oil recovery of low permeability reservoirs. At present, nanofluids have encountered some difficulties in increasing production, such as poor stability and high cost.

[0003] In order to solve the problems of poor stability and high cost of nanofluids, many scholars have made a lot of attempts. For example, Liang et al. used molybdenum disulfide modified with octylamine to prepare amphiphilic nanosheets with good stability, thereby preparing AP-MDN nanofluids and obtaining an oil reservoir recovery rate of 19.1%. Jia et al. proposed an innovative composite membrane nanofluid system, combining modified bacterial nanofibers with boron nitride nanosheets to increase the surface charge density of the nanosheets, thereby preparing stable nanofluids. Li et al. used 8-cyclodextrin (8-CD) grafted SiO2 nanoparticles to prepare 8-CD-SiO2 nanofluids, showing excellent stability and salt resistance. Morteza Mansouri Zadeh et al. synthesized stable silica nanoparticles in aqueous phase through a sol-gel process, increasing the secondary recovery rate by 13.7%. Liu et al. selected the biocompatible reducing agent "ascorbic acid" to prepare nanosilver, and synthesized biogenic nanosilver composites using fungal fermentation supernatant to enhance crude oil recovery. Sumadi Paryoto et al. prepared a stable Fe3O4 nanofluid by using composite surfactants and Fe3O4 nanoparticles. BilaA et al. tried to stabilize nano-SiO2 by bonding or coating macromolecules (such as polymers) on the surface of nanoparticles or modifying nanoparticles. Sagala et al. prepared a stable nanofluid using surfactant-coated nanomaterials. Bhuvanesh et al. prepared AGO / HPAM nanofluid using AGO nanocomposites of different concentrations, which increased the oil reservoir recovery by 15.7% compared with pure polymer displacement. Li et al. synthesized carbon nanodots (CDs) by hydrothermal reaction, and prepared activated carbon nanodots (sm-CDs) by surface modification, which enhanced the oil recovery. Tian et al. prepared amphoteric titanium dioxide nanofluid by chemical reaction of nano-titanium dioxide (NTD) and titanium ester coupling agent, and dispersed it using Span85 dispersant. The nanofluid displacement technology increased the oil reservoir recovery by 26.4%. Zhao et al. combined hydrophilic silica sol with 0.1wt% of the modifier lauryl amide propyl hydroxysulfonate to prepare stable functional silicon nanofluids that can withstand high salt and high temperature environments.

[0004] The above methods can be mainly divided into two categories. One is to use surfactants or polymers as stabilizers to prepare stable nanofluids. The other is to modify the surface of nanoparticles to make them have the same surface charge and use electrostatic repulsion to stabilize the nanofluid. However, the stability of the nanofluid prepared by the above method is still poor. Therefore, a method for preparing a nanofluid with good stability is urgently needed. Summary of the invention

[0005] The object of the present invention is to provide a calcium carbonate nanofluid and a preparation method and application thereof. The calcium carbonate nanofluid prepared by the present invention has excellent stability.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a calcium carbonate nanofluid, comprising the following steps:

[0008] (1) mixing hydrolyzed polymaleic anhydride, water and alkali solution for neutralization reaction to obtain a mixed solution;

[0009] (2) adding a soluble calcium salt solution and a soluble carbonate solution dropwise to the mixed solution obtained in step (1) to carry out a chelating precipitation reaction to obtain a calcium carbonate nanofluid.

[0010] Preferably, in the step (1), the volume ratio of the hydrolyzed polymaleic anhydride to water is (0.01-0.2):1.

[0011] Preferably, the pH value of the mixed system obtained by mixing water and alkali solution in step (1) is 9-13.

[0012] Preferably, the soluble calcium salt solution in step (2) comprises one or more of an aqueous solution of calcium chloride, an aqueous solution of calcium nitrate and an aqueous solution of calcium acetate.

[0013] Preferably, the soluble carbonate solution in step (2) comprises one or both of a sodium carbonate aqueous solution and a potassium carbonate aqueous solution.

[0014] Preferably, the concentration of the soluble calcium salt solution in step (2) is 0.5 to 2 mol / L.

[0015] Preferably, the volume ratio of the soluble calcium salt solution in step (2) to the hydrolyzed polymaleic anhydride in step (1) is (1-20):1.

[0016] Preferably, the molar ratio of calcium ions in the soluble calcium salt solution to carbonate ions in the soluble carbonate solution in step (2) is (0.9-1.1):1.

[0017] The present invention also provides a calcium carbonate nanofluid prepared by the preparation method described in the above technical solution.

[0018] The present invention also provides the application of the calcium carbonate nanofluid described in the above technical solution in oil field exploitation.

[0019] The present invention provides a preparation method of calcium carbonate nanofluid, comprising the following steps: (1) mixing hydrolyzed polymaleic anhydride, water and alkali solution for neutralization reaction to obtain a mixed solution; (2) dropping a soluble calcium salt solution and a soluble carbonate solution into the mixed solution obtained in the step (1) for chelation precipitation reaction to obtain a calcium carbonate nanofluid. The present invention mixes hydrolyzed polymaleic anhydride, water and alkali solution for neutralization reaction, so that the carboxyl group in the hydrolyzed polymaleic anhydride is converted into a carboxylate radical, which is convenient for subsequent chelation with calcium ions; dropping a soluble calcium salt solution and a soluble carbonate solution into the mixed solution for chelation precipitation reaction; during the reaction, the calcium ions chelate with the hydrolyzed polymaleic anhydride on the one hand, and react with carbonate radicals on the other hand to form calcium carbonate, thereby forming a calcium carbonate nanofluid; the stability of the nanofluid is improved through the synchronous chelation precipitation reaction; the nanofluid has good interfacial tension reduction performance and emulsification, and has excellent reservoir recovery when used as an oil displacement agent for oil field exploitation. The results of the examples show that 46% of the calcium carbonate nanofluid prepared by the present invention remains unprecipitated after standing for 10 days, while the pure calcium carbonate nanofluid is completely precipitated on the first day, and the nanofluid obtained by directly mixing calcium carbonate and hydrolyzed polymaleic anhydride is also completely precipitated after stopping stirring. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram of the process for preparing the calcium carbonate nanofluid in Example 1 of the present invention;

[0021] Figure 2 This is a diagram showing the stability mechanism of the calcium carbonate nanofluid in Example 1 of the present invention;

[0022] Figure 3 The infrared spectra of the calcium carbonate nanofluid prepared in Example 1 of the present invention and the calcium carbonate nanofluid prepared in Comparative Example 1;

[0023] Figure 4 Thermogravimetric curves of the calcium carbonate nanofluid prepared in Example 1 of the present invention and the calcium carbonate nanofluid prepared in Comparative Example 1;

[0024] Figure 5 The oil-water interfacial tension diagram of the calcium carbonate nanofluid prepared in Example 1 of the present invention, the calcium carbonate nanofluid prepared in Comparative Example 1, and deionized water;

[0025] Figure 6 This is an emulsification index diagram of the calcium carbonate nanofluid prepared in Example 1 of the present invention at different concentrations;

[0026] Figure 7 This is a macroscopic image of the calcium carbonate nanofluid prepared in Example 1 of the present invention after being left standing at room temperature for 1 to 10 days;

[0027] Figure 8This is a macroscopic image of the calcium carbonate nanofluid prepared in Comparative Example 1 after being left standing at room temperature for 1 to 10 days;

[0028] Fig. 9 The stability diagram of the calcium carbonate nanofluid prepared in Example 1 of the present invention and the calcium carbonate nanofluid prepared in Comparative Example 2;

[0029] Fig.10 This is a graph showing the displacement experiment of the calcium carbonate nanofluid prepared in Example 1 of the present invention;

[0030] Fig.11 This is a diagram showing the mechanism of improving oil recovery of the calcium carbonate nanofluid prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The present invention provides a method for preparing a calcium carbonate nanofluid, comprising the following steps:

[0032] (1) mixing hydrolyzed polymaleic anhydride, water and alkali solution for neutralization reaction to obtain a mixed solution;

[0033] (2) adding a soluble calcium salt solution and a soluble carbonate solution dropwise to the mixed solution obtained in step (1) to carry out a chelating precipitation reaction to obtain a calcium carbonate nanofluid.

[0034] Unless otherwise specified, the present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.

[0035] The invention mixes hydrolyzed polymaleic anhydride, water and alkali solution and then performs neutralization reaction to obtain a mixed solution.

[0036] In the present invention, the average molecular weight of the hydrolyzed polymaleic anhydride is preferably 400-600, more preferably 500. The present invention limits the average molecular weight of the hydrolyzed polymaleic anhydride to the above range, which can make it have a suitable carbon chain length, have better steric hindrance effect, and further improve the stability of the calcium carbonate nanofluid.

[0037] In the present invention, the volume ratio of the hydrolyzed polymaleic anhydride to water is preferably (0.01-0.2): 1, more preferably (0.02-0.15): 1. The present invention limits the volume ratio of the hydrolyzed polymaleic anhydride to water to the above range, so that the raw materials can be fully dissolved.

[0038] In the present invention, the alkali solution preferably includes a sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution. In the present invention, the concentration of the alkali solution is preferably 1 to 3 mol / L, more preferably 2 mol / L.

[0039] In the present invention, the mixing of the hydrolyzed polymaleic anhydride, water and alkali solution is preferably carried out by mixing water and alkali solution to obtain a mixed system, and then adding the hydrolyzed polymaleic anhydride.

[0040] In the present invention, the pH value of the mixed system obtained by mixing the water and the alkali solution is preferably 9 to 13, more preferably 10 to 13. The present invention has no special limitation on the amount of the alkali solution, as long as the pH value of the mixed system is within the above range. The present invention limits the pH value of the mixed system within the above range, which is more conducive to hydrolyzing the carboxyl groups in the polymaleic anhydride into carboxyl groups, and is more conducive to the subsequent chelation with calcium ions.

[0041] In the present invention, the temperature of the neutralization reaction is preferably 20-30° C. In the present invention, the neutralization reaction starts when the hydrolyzed polymaleic anhydride is added, and the process of adding and mixing the hydrolyzed polymaleic anhydride is the process of the neutralization reaction. In the present invention, during the neutralization reaction, the carboxyl groups in the hydrolyzed polymaleic anhydride react under alkaline conditions to form carboxyl groups.

[0042] After obtaining the mixed solution, the present invention drips the soluble calcium salt solution and the soluble carbonate solution into the mixed solution to carry out a chelating precipitation reaction to obtain a calcium carbonate nanofluid.

[0043] In the present invention, the soluble calcium salt solution preferably includes one or more of a calcium chloride aqueous solution, a calcium nitrate aqueous solution and a calcium acetate aqueous solution, and more preferably a calcium chloride aqueous solution.

[0044] In the present invention, the concentration of the soluble calcium salt solution is preferably 0.5-2 mol / L, more preferably 1 mol / L. The present invention limits the concentration of the soluble calcium salt solution to the above range, which can make the calcium salt fully dissolved and have a suitable chelation precipitation rate subsequently, further improving the stability of the calcium carbonate nanofluid.

[0045] In the present invention, the volume ratio of the soluble calcium salt solution to the hydrolyzed polymaleic anhydride is preferably (1-20): 1, more preferably 10: 1. The present invention limits the volume ratio of the soluble calcium salt solution to the hydrolyzed polymaleic anhydride within the above range, which can make the surface of calcium carbonate chelate more hydrolyzed polymaleic anhydride, further improving the stability of the calcium carbonate nanofluid.

[0046] In the present invention, the soluble carbonate solution preferably includes one or both of a sodium carbonate aqueous solution and a potassium carbonate aqueous solution, and more preferably a sodium carbonate aqueous solution.

[0047] In the present invention, the concentration of the soluble carbonate solution is preferably 0.5-2 mol / L, more preferably 1 mol / L. The present invention limits the concentration of the soluble carbonate solution to the above range, which can fully dissolve the carbonate and subsequently have a suitable chelation precipitation rate, further improving the stability of the calcium carbonate nanofluid.

[0048] In the present invention, the volume ratio of the soluble carbonate solution to the hydrolyzed polymaleic anhydride is preferably (1-20): 1, more preferably 10: 1. The present invention limits the volume ratio of the soluble carbonate solution to the hydrolyzed polymaleic anhydride within the above range, which can make the surface of calcium carbonate chelate more hydrolyzed polymaleic anhydride, further improving the stability of the calcium carbonate nanofluid.

[0049] In the present invention, the volume ratio of the soluble calcium salt solution to the soluble carbonate solution is preferably (0.9-1.1):1, more preferably 1:1; the molar ratio of calcium ions in the soluble calcium salt solution to carbonate ions in the soluble carbonate solution is preferably (0.9-1.1):1, more preferably 1:1. The present invention limits the molar ratio of calcium ions in the soluble calcium salt solution to carbonate ions in the soluble carbonate solution to the above range, so that the two can fully react to generate calcium carbonate.

[0050] In the present invention, the drop rate of the soluble calcium salt solution and the soluble carbonate solution is preferably the same. In the present invention, the drop rate of the soluble calcium salt solution and the soluble carbonate solution is preferably 0.5 to 5 mL / min. The present invention simultaneously drops the soluble calcium salt solution and the soluble carbonate solution and limits the drop rate of both, so that the chelation and precipitation reactions can be fully carried out, and the stability of the calcium carbonate nanofluid is further improved.

[0051] In the present invention, the soluble calcium salt solution and the soluble carbonate solution are preferably placed in a constant pressure funnel for dropwise addition. The constant pressure funnel used in the present invention is conducive to the dropwise addition process.

[0052] In the present invention, the temperature of the chelate precipitation reaction is preferably 40-100°C, more preferably 60-80°C; the time of the chelate precipitation reaction is preferably 1-24h, more preferably 1-5h; the chelate precipitation reaction is preferably carried out under stirring; the stirring rate is preferably 700-900r / min, more preferably 800r / min. In the present invention, the chelate precipitation reaction starts when the soluble calcium salt solution and the soluble carbonate solution are added dropwise. In the present invention, during the chelate precipitation reaction, calcium ions chelate with hydrolyzed polymaleic anhydride on the one hand, and react with carbonate to form calcium carbonate on the other hand, thereby forming calcium carbonate nanofluid. The present invention limits the temperature and time of the chelate precipitation reaction within the above range, which can make the reaction more sufficient.

[0053] After the chelating precipitation reaction is completed, the present invention preferably cools the product of the chelating precipitation reaction to obtain a calcium carbonate nanofluid.

[0054] The present invention has no special limitation on the cooling operation, and cooling to room temperature may be performed using cooling technical solutions well known to those skilled in the art.

[0055] The invention mixes hydrolyzed polymaleic anhydride, water and alkali solution and then performs a neutralization reaction, so that the carboxyl group in the hydrolyzed polymaleic anhydride is converted into a carboxylate group, which is convenient for subsequent chelation with calcium ions. A soluble calcium salt solution and a soluble carbonate solution are dripped into the mixed solution to perform a chelation precipitation reaction. During the reaction, the calcium ions chelate with the hydrolyzed polymaleic anhydride on the one hand, and react with the carbonate group on the other hand to form calcium carbonate, thereby forming a calcium carbonate nanofluid. The stability of the nanofluid is improved through the synchronous chelation precipitation reaction, and the nanofluid has good interfacial tension reduction performance and emulsification. When used as an oil displacement agent for oil field exploitation, the nanofluid has an excellent reservoir recovery rate.

[0056] The present invention also provides a calcium carbonate nanofluid prepared by the preparation method described in the above technical solution.

[0057] The calcium carbonate nanofluid prepared by the invention has excellent stability, performance of reducing interfacial tension and emulsification, and has excellent oil reservoir recovery rate when used as an oil displacement agent in oil field exploitation.

[0058] The present invention also provides the application of the calcium carbonate nanofluid described in the above technical solution in oil field exploitation.

[0059] The present invention has no special limitation on the operation of the application, and the technical solutions of the application well known to those skilled in the art may be adopted.

[0060] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] Example 1

[0062] (1) At room temperature, 200 mL of deionized water was added to a three-necked flask, 20 mL of a 2 mol / L sodium hydroxide aqueous solution was added to adjust the pH value of the mixed system to 13, and then 5 mL of hydrolyzed polymaleic anhydride (average molecular weight 500) was added to obtain a mixed solution (the volume ratio of hydrolyzed polymaleic anhydride to deionized water was 0.025:1);

[0063] (2) 50 mL of 1 mol / L calcium chloride aqueous solution and 50 mL of 1 mol / L sodium carbonate aqueous solution were placed in a constant pressure funnel respectively, and then placed in the two necks of a three-necked flask, and the calcium chloride aqueous solution and the sodium carbonate aqueous solution were added dropwise to the three-necked flask at the same rate (the dropping rate was 1 mL / min, the volume ratio of the calcium chloride aqueous solution to the sodium carbonate aqueous solution was 1:1, the molar ratio of calcium ions in the calcium chloride aqueous solution to carbonate ions in the sodium carbonate aqueous solution was 1:1, and the volume ratio of the calcium chloride aqueous solution to the hydrolyzed polymaleic anhydride was 10:1), and the reaction was carried out at 60° C. with stirring for 1 h at a stirring rate of 800 r / min, and then cooled to obtain a calcium carbonate nanofluid, which was recorded as CaCO3-HPMA.

[0064] Example 2

[0065] (1) At room temperature, 80 mL of deionized water was added to a three-necked flask, 6 mL of a 2 mol / L sodium hydroxide aqueous solution was added to adjust the pH value of the mixed system to 12.5, and then 6 mL of hydrolyzed polymaleic anhydride (average molecular weight 500) was added to obtain a mixed solution (the volume ratio of hydrolyzed polymaleic anhydride to deionized water was 0.075:1);

[0066] (2) 50 mL of 1 mol / L calcium chloride aqueous solution and 50 mL of 1 mol / L sodium carbonate aqueous solution were placed in a constant pressure funnel respectively, and then placed in the two necks of a three-necked flask, and the calcium chloride aqueous solution and the sodium carbonate aqueous solution were added dropwise to the three-necked flask at the same rate (the dropping rate was 0.5 mL / min, the volume ratio of the calcium chloride aqueous solution to the sodium carbonate aqueous solution was 1:1, the molar ratio of calcium ions in the calcium chloride aqueous solution to carbonate ions in the sodium carbonate aqueous solution was 1:1, and the volume ratio of the calcium chloride aqueous solution to the hydrolyzed polymaleic anhydride was 8.3:1), and the reaction was carried out at 60° C. with stirring for 1 h at a stirring rate of 800 r / min, and then cooled to obtain a calcium carbonate nanofluid.

[0067] Example 3

[0068] (1) At room temperature, 100 mL of deionized water was added to a three-necked flask, 9 mL of a 2 mol / L sodium hydroxide aqueous solution was added to adjust the pH value of the mixed system to 13, and then 6 mL of hydrolyzed polymaleic anhydride (average molecular weight 500) was added to obtain a mixed solution (the volume ratio of hydrolyzed polymaleic anhydride to deionized water was 0.06:1);

[0069] (2) 50 mL of a 1 mol / L calcium chloride aqueous solution and 50 mL of a 1 mol / L sodium carbonate aqueous solution were placed in a constant pressure funnel, respectively, and then placed in the two necks of a three-necked flask, and the calcium chloride aqueous solution and the sodium carbonate aqueous solution were added dropwise to the three-necked flask at the same rate (the dropping rate was 2.0 mL / min, the volume ratio of the calcium chloride aqueous solution to the sodium carbonate aqueous solution was 1:1, the molar ratio of calcium ions in the calcium chloride aqueous solution to carbonate ions in the sodium carbonate aqueous solution was 1:1, and the volume ratio of the calcium chloride aqueous solution to the hydrolyzed polymaleic anhydride was 8.3:1), and the mixture was reacted at 70° C. for 1 h at a stirring rate of 800 r / min, and then cooled to obtain a calcium carbonate nanofluid.

[0070] Comparative Example 1

[0071] The hydrolysis of polymaleic anhydride in Example 1 was omitted to obtain a calcium carbonate nanofluid, which was denoted as CaCO3.

[0072] Comparative Example 2

[0073] The calcium carbonate nanofluid prepared in Comparative Example 1 was mixed with hydrolyzed polymaleic anhydride (the mass ratio of calcium carbonate to hydrolyzed polymaleic anhydride was 1:1) to obtain a calcium carbonate nanofluid with a concentration of 15 g / L.

[0074] Example 1 The schematic flow diagram of the preparation method of calcium carbonate nanofluid is preferably as follows Figure 1 shown.

[0075] The stability mechanism diagram of the calcium carbonate nanofluid prepared in Example 1 is as follows Figure 2 As shown in Figure 3, the excellent stability of CaCO3-HPMA nanofluids is due to the fact that, on the one hand, the huge steric hindrance of hydrolyzed polymaleic anhydride offsets part of the van der Waals attraction, and on the other hand, sodium carboxylate carries a negative charge in aqueous solution. The electrostatic repulsion of CaCO3-HPMA is sufficient to offset the aggregation caused by van der Waals forces.

[0076] The infrared spectra of the CaCO3-HPMA nanofluid prepared in Example 1 and the CaCO3 nanofluid prepared in Comparative Example 1 are as follows: Figure 3 As shown. Figure 3 As can be seen, 713.2cm -1 and 858.1cm -1 The peak at 1090.1 cm is attributed to the bending vibration of the CO bond. -1 and 1477.2cm -1 The peaks correspond to the symmetric and antisymmetric stretching vibrations of the CO bond, 3432.6 cm -1 The peak at 2929.3 cm represents the stretching vibration of the hydroxyl group from bound water. -1 and 2850.2cm -1The peak at 1798.9 cm represents the stretching vibration of the CC bond, while the peak at 1798.9 cm -1 and 1710.6cm -1 The peaks of are assigned to the antisymmetric and symmetric stretching vibrations of the C=O bond. These results confirm that CaCO3-HPMA was successfully synthesized.

[0077] The thermogravimetric curves of the CaCO3-HPMA nanofluid prepared in Example 1 and the CaCO3 nanofluid prepared in Comparative Example 1 are as follows: Figure 4 As shown. Figure 4 It can be seen that the mass loss process is divided into three stages. In the first stage, from 27 to 100 ° C, the mass loss rate of CaCO3-HPMA is 1.0%, and the mass loss rate of CaCO3 is 0.01%, which is mainly attributed to the evaporation of water molecules adsorbed on the surface of CaCO3 and CaCO3-HPMA. Compared with CaCO3, CaCO3-HPMA has more hydrophilic groups and can adsorb more water, thus resulting in more mass loss. In the second stage, from 100 ° C to 530 ° C, the mass loss rate of CaCO3-HPMA is 14.2%, and that of CaCO3 is 0.0%. The significant increase in the mass loss of CaCO3-HPMA is attributed to the decomposition of HPMA grafted on the surface of CaCO3-HPMA. When the temperature exceeds 530 ° C and enters the third stage, the mass loss rate of CaCO3-HPMA is 10.3%, and that of CaCO3 is 15.2%. The significant increase in the mass loss of CaCO3 and CaCO3-HPMA is attributed to the thermal decomposition of CaCO3.

[0078] The interfacial tension between the CaCO3-HPMA nanofluid prepared in Example 1 and the CaCO3 nanofluid prepared in Comparative Example 1 and deionized water was measured using the hanging drop method. The CaCO3-HPMA nanofluid and the CaCO3 nanofluid were dispersed in deionized water to prepare 1000 mg / L of nanofluid, with kerosene as the oil phase. The interfacial tension between the nanofluid and kerosene was measured at 60°C. The measurement was performed every 10 seconds, and the steady-state interfacial tension values ​​within 600 seconds were recorded. The results are shown in FIG. Figure 5 As shown. Figure 5 It can be seen that the interfacial tension of oil and water decreases with the increase of time. At 600s, the interfacial tension of oil and water changes little, which shows that the prepared CaCO3-HPMA nanofluid has a good performance in reducing interfacial tension.

[0079] The CaCO3-HPMA nanofluid prepared in Example 1 was dispersed in deionized water to prepare nanofluids of different concentrations (250 mg / L, 500 mg / L, 1000 mg / L). The nanofluid (10 mL) and kerosene (10 mL) were added to a glass bottle, emulsified at a speed of 10000 r / min for 2 minutes using an emulsifier, and then placed at 60°C for observation. The emulsification index is the ratio of the emulsified volume to the total volume after standing for 24 to 240 hours. The higher the emulsification index, the better the emulsification effect. The results are as follows: Figure 6 As shown. Figure 6 It can be seen that the emulsification performance of CaCO3-HPMA nanofluid increases with increasing concentration, but decreases over time. For CaCO3-HPMA nanofluid (250 mg / L), the emulsification index is 10% after 240 hours at 60°C. For CaCO3-HPMA nanofluid (500 mg / L), the emulsification index is 15% after 240 hours at 60°C. For CaCO3-HPMA nanofluid (1000 mg / L), the emulsification index is 20% after 240 hours at 60°C. This shows that CaCO3-HPMA nanofluid has excellent emulsification properties.

[0080] The CaCO3-HPMA nanofluid (15 g / L) prepared in Example 1 and the CaCO3 nanofluid (15 g / L) prepared in Comparative Example 1 were allowed to stand at room temperature to evaluate their stability. The results were as follows: Figure 7 and Figure 8 As shown. Figures 7-8 As can be seen in the figure, after standing at room temperature for 10 days, 46% of the CaCO3-HPMA nanofluid (15 g / L) was still unprecipitated, indicating its relatively good stability. In contrast, the CaCO3 nanofluid (15 g / L) was completely precipitated on the first day.

[0081] The CaCO3-HPMA nanofluid (15 g / L) prepared in Example 1 and the CaCO3 nanofluid (15 g / L) prepared in Comparative Example 2 were allowed to stand at room temperature to evaluate their stability. Fig. 9 As shown, Fig. 9 (a) is a macroscopic image of the CaCO3-HPMA nanofluid prepared in Example 1, and (b) is a schematic structural diagram of the CaCO3-HPMA nanofluid prepared in Example 1; (c) is a macroscopic image of the CaCO3 nanofluid prepared in Comparative Example 2, and (d) is a schematic structural diagram of the CaCO3 nanofluid prepared in Comparative Example 2. Fig. 9It can be seen that the stability of the nanofluid (concentration of 15 g / L) prepared by mixing CaCO3 nanoparticles and HPMA in Comparative Example 2 is poor. After stopping stirring, the CaCO3 nanoparticles are almost all precipitated at the bottom of the measuring cylinder after being poured into the measuring cylinder. This is mainly because there are very few calcium ions on the surface of the calcium carbonate nanoparticles, which are almost difficult to chelate with the hydrolyzed polymaleic anhydride HPMA. The calcium carbonate nanoparticles settle under the action of gravity. In the preparation method of Example 1 of the present invention, the CaCO3 nanoparticles are 2+ On the one hand, it will chelate with HPMA, and on the other hand, it will chelate with CO3 2- The reaction generates CaCO3. The two reactions are combined to prepare CaCO3-HPMA nanofluids. First, CaCO3-HPMA is negatively charged in aqueous solution, and CaCO3-HPMA carries the same charge. Secondly, HPMA grafted on the surface of CaCO3-HPMA has a certain steric hindrance, which can increase the stability of CaCO3-HPMA nanofluids. CaCO3-HPMA stabilizes nanofluids by electrostatic repulsion.

[0082] Application Examples

[0083] In order to explore the ability of the CaCO3-HPMA nanofluid prepared in Example 1 to improve the permeability of low-permeability reservoirs, an oil displacement experiment was conducted. The permeability of the simulated reservoir was 15.2×10 -3 μm 2 The core parameters and the results of the enhanced oil recovery of the CaCO3-HPMA nanofluid prepared in Example 1 are shown in Tables 1 and Fig.10 The mechanism diagram of CaCO3-HPMA nanofluid for improving oil recovery is shown in Fig.11 shown.

[0084] Table 1 Core parameters and results of enhanced oil recovery of CaCO3-HPMA nanofluid prepared in Example 1

[0085]

[0086] From Table 1 and Fig.10It can be seen that the injection pressure of the simulated formation rose rapidly after the first water flooding. After the injection of CaCO3-HPMA nanofluid flooding, the injection pressure of the simulated formation decreased. After the second water flooding, the injection pressure increased slightly and finally stabilized at 3.8MPa. After the injection of 0.5PV CaCO3-HPMA nanofluid, the nanofluid and the subsequent second water flooding increased the recovery factor by 14.0%. This shows that CaCO3-HPMA nanofluid flooding can improve the recovery factor of low permeability reservoirs. The water content continued to rise after the first water flooding, and the water content decreased significantly after the CaCO3-HPMA nanofluid flooding, further indicating that CaCO3-HPMA nanofluid can improve the recovery factor of medium and low permeability reservoirs. On the one hand, this is due to the fact that nanomaterials will form a wedge-shaped area at the three-phase interface of rock / crude oil / injection fluid during the flooding process, and the wedge-shaped squeezing effect is used to improve the crude oil recovery factor. On the other hand, thanks to the amphiphilicity of CaCO3-HPMA, it can reduce the oil-water interfacial tension, emulsify crude oil, and transform the oil-wet reservoir into a water-wet reservoir, which is conducive to water flooding.

[0087] CaCO3-HPMA has an amphiphilic structure, large specific surface area and high surface energy, and can be better adsorbed at the oil-water interface to form a thin film. Fig.11 The mechanism by which CaCO3-HPMA nanofluids improve oil recovery efficiency is demonstrated, and the mechanism by which CaCO3-HPMA nanofluids improve oil recovery efficiency can be attributed to four key factors. First, the surface of reservoir rocks is mainly oil-wet or mixed wettability. When CaCO3-HPMA nanofluid contacts the rock, it transforms the surface into a hydrophilic or neutral wettability state. This change reduces the resistance to the movement of oil droplets, making water flooding easier and improving oil recovery efficiency. Second, a wedge-shaped region is formed at the interface of rock, crude oil, and injected liquid. This region generates a forward force through Brownian motion and electrostatic interaction, effectively stripping the crude oil from the rock and improving oil recovery efficiency. Third, CaCO3-HPMA nanofluids reduce the oil-water interfacial tension and help the oil film detach. Fourth, CaCO3-HPMA nanofluids emulsify the crude oil, breaking it up into smaller oil droplets, making it easier to be carried away.

[0088] In summary, the calcium carbonate nanofluid prepared by the present invention has excellent stability, and the nanofluid has good performance in reducing interfacial tension and emulsification, and has excellent oil reservoir recovery when used as an oil displacement agent in oil field exploitation.

[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a calcium carbonate nanofluid, comprising the following steps: (1) mixing hydrolyzed polymaleic anhydride, water and alkali solution for neutralization reaction to obtain a mixed solution; (2) adding a soluble calcium salt solution and a soluble carbonate solution dropwise to the mixed solution obtained in step (1) to carry out a chelating precipitation reaction to obtain a calcium carbonate nanofluid.

2. The preparation method according to claim 1, characterized in that: In the step (1), the volume ratio of hydrolyzed polymaleic anhydride to water is (0.01-0.2):

1.

3. The preparation method according to claim 1, characterized in that: The pH value of the mixed system obtained by mixing water and alkali solution in step (1) is 9-13.

4. The preparation method according to claim 1, characterized in that: The soluble calcium salt solution in step (2) includes one or more of a calcium chloride aqueous solution, a calcium nitrate aqueous solution and a calcium acetate aqueous solution.

5. The preparation method according to claim 1, characterized in that: The soluble carbonate solution in step (2) includes one or both of a sodium carbonate aqueous solution and a potassium carbonate aqueous solution.

6. The preparation method according to claim 1, characterized in that: The concentration of the soluble calcium salt solution in step (2) is 0.5-2 mol / L.

7. The preparation method according to claim 6, characterized in that: The volume ratio of the soluble calcium salt solution in step (2) to the hydrolyzed polymaleic anhydride in step (1) is (1-20):

1.

8. The preparation method according to claim 1, characterized in that: The molar ratio of calcium ions in the soluble calcium salt solution to carbonate ions in the soluble carbonate solution in step (2) is (0.9-1.1):

1.

9. The calcium carbonate nanofluid prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the calcium carbonate nanofluid according to claim 9 in oil field exploitation.

Citation Information

Patent Citations

  • Calcium sequestering composition

    CN103649290A

  • Process for producing calcitic spheroidal calcium carbonate and synergistic dentifrice composition obtained using calcitic spheroidal calcium carbonate

    IN189828B

  • Process for producing acid-type maleic acid polymer and water-treating agent and detergent additive containing said polymer

    US5135677A

  • Method of inhibiting scale formation

    US6146538A

  • Composite microparticles and production method for same

    WO2011115280A1