Method for synergistically improving performance of electrode material by utilizing co-doping of aluminum / potassium elements

Through the one-step calcining process of aluminum/potassium element co-doping, the problem of poor circulation and rate performance of lithium-rich manganese-based positive electrode materials is solved, and efficient and simple electrochemical performance is achieved, reducing production costs, and aluminum doping is achieved. The cycling performance is best when the amount is 3%, and the rate performance is significantly improved when the potassium doping amount is 3%.

CN119059577APending Publication Date: 2024-12-03NANJING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411191763.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The circulation and rate performance of lithium-rich manganese-based cathode materials are poor. The existing improvement strategies require the superposition of multi-step modification strategies, which increases production costs and lacks an efficient and simple one-step method.

Method used

Through the method of co-doping of aluminum/potassium elements, aluminum ions are used to stabilize the crystal lattice and potassium ions to broaden the layer spacing, and a one-step calcination process is used to improve the cyclic performance and rate performance of the electrode material.

Benefits of technology

It achieves simple and efficient cycling and rate performance of lithium-rich manganese-based positive electrode materials simultaneously, reducing production costs, the best effect is when the aluminum doping amount is 3%, and the rate performance is significantly improved when the potassium doping amount is 3%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059577A_ABST
    Figure CN119059577A_ABST
Patent Text Reader

Abstract

The invention discloses a method for synergistically improving the performance of an electrode material by utilizing co-doping of aluminum / potassium elements, which comprises the following steps: adding aluminum hydroxide and potassium hydroxide when a lithium-rich manganese-based positive electrode material precursor and lithium carbonate are ground and mixed, and then carrying out high-temperature calcination to prepare the lithium-rich manganese-based positive electrode material. According to the invention, the aluminum / potassium co-doping synergistic effect is utilized, the respective advantages of the two doping elements are exerted, and meanwhile, the cycle performance and the rate capability of the electrode material are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a method for synergistically improving electrode material performance by co-doping with aluminum / potassium elements. Background Art

[0002] With the increasing development of new energy technologies, people's demand for electric vehicles driven by lithium-ion batteries is increasing. On the one hand, power batteries currently account for a large proportion of the cost of new energy vehicles. If the electrochemical performance of power batteries cannot be maintained stable during repeated charging and discharging, frequent battery replacement will bring a great burden to consumers; on the other hand, with the acceleration of people's pace of life, the charging time of electric vehicles is also a focus of people's attention. Effectively improving the fast charging and discharging performance of power batteries is also one of the directions of future efforts. It can be seen that improving the cycle performance and fast charging and discharging performance (rate performance) of power batteries is an urgent need at present.

[0003] As a high-capacity, high-operating-voltage electrode material, lithium-rich manganese-based cathode materials may be one of the candidates for high-energy-density power battery cathode materials in the future. However, due to problems such as non-oxidative loss and structural phase change, the cycle performance and rate performance of lithium-rich manganese-based cathode materials are poor. In order to meet the needs of the future power battery market, improving its cycle performance and rate performance through effective strategies is one of the current focuses of electrode material modification.

[0004] A common strategy to improve the cycle performance of lithium-rich manganese-based positive electrode materials is the coating strategy, which usually uses a corrosion-resistant coating layer to coat the surface of the positive electrode material to prevent the electrolyte from corroding it; and a common method to improve the rate performance of lithium-rich manganese-based positive electrode materials is to compound them with carbon materials with excellent conductivity, such as carbon nanotubes, graphene, etc. It can be seen that for unmodified positive electrode materials, in order to improve their cycle performance and rate performance at the same time, it is necessary to superimpose multiple modification strategies on the electrode materials (coating strategy + carbon material composite), which is likely to further increase production costs. It is currently urgently needed to develop an efficient and simple one-step modification strategy to effectively improve the electrochemical properties of lithium-rich manganese-based positive electrode materials at the same time. Summary of the invention

[0005] In order to improve the cycle performance and rate performance of positive electrode materials efficiently and simply at the same time, the present invention provides a method for synergistically improving the performance of electrode materials by co-doping with aluminum / potassium elements.

[0006] The technical solution to achieve the purpose of the present invention is: a method for improving the performance of electrode materials by co-doping with aluminum / potassium elements, comprising the following steps:

[0007] (1) mixing and grinding a lithium-rich manganese-based positive electrode material precursor, lithium carbonate, potassium hydroxide and aluminum hydroxide uniformly;

[0008] (2) The obtained precursor mixture is first calcined at 500±20°C for 6 hours and then heated to 850±20°C for 14 hours to obtain a lithium-rich manganese-based positive electrode material.

[0009] Preferably, the precursor of the lithium-rich manganese-based positive electrode material is Mn 0.54 Co 0.13 Ni 0.13 CO3.

[0010] Preferably, the mass ratio of the lithium-rich manganese-based positive electrode material precursor to lithium carbonate is 1:0.4387.

[0011] Preferably, the molar ratio of potassium hydroxide to lithium carbonate is 3%, ie, n(K):n(Li)=1.5%.

[0012] Preferably, the molar ratio of aluminum hydroxide to lithium carbonate is 3%, that is, n(Al):n(Li)=1.5%.

[0013] Preferably, the heating rate and the cooling rate are both 5°C / min.

[0014] Compared with the prior art, the present invention has the following positive effects:

[0015] (1) The present invention uses a one-step aluminum / potassium synergistic co-doping method to efficiently and simultaneously improve the cycle performance and rate performance of lithium-rich manganese-based positive electrode materials, wherein aluminum ions help improve the cycle performance of electrode materials by stabilizing lattice oxygen, and potassium ions help improve the rate performance of electrode materials by widening the interlayer spacing;

[0016] (2) The modification process of the present invention is simple and efficient, which reduces production costs and achieves multiple electrochemical performance improvements. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the performance diagram of LMO, LMO-Al1, LMO-Al3, and LMO-Al5 after 100 cycles at 1C.

[0018] Figure 2 This is a schematic diagram of the discharge medium voltage of LMO, LMO-Al1, LMO-Al3, and LMO-Al5 after 100 cycles at 1C.

[0019] Figure 3 (a) Ni 2p, (b) Co 2p, (c) Mn 2p and (d) O 1s XPS spectra of LMO and LMO-Al3.

[0020] Figure 4 This is the rate performance diagram of LMO, LMO-K1, LMO-K3, and LMO-K5.

[0021] Figure 5 (a) Ni 2p, (b) Co 2p, (c) Mn 2p, and (d) O 1s XPS spectra of LMO and LMO-K3.

[0022] Figure 6 This is the performance diagram of LMO, LMO-Al3, LMO-K3, and LMO-Al+K after 100 cycles at 1C.

[0023] Figure 7 It is the XRD spectra of LMO, LMO-Al3, LMO-K3, LMO-Al+K and the enlarged images of (003) and (101) peaks.

[0024] Figure 8 This is the rate performance diagram of LMO, LMO-Al3, LMO-K3, and LMO-Al+K. DETAILED DESCRIPTION

[0025] The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0026] The inventive concept of the present invention is: the present invention utilizes the characteristics of different cations to synergistically co-dope the positive electrode material, wherein the cation characteristics include ion radius, ion valence, etc. + Compared to Li + The larger ion radius broadens the lithium ion diffusion channel; using Al 3+ It is easy to form a stronger metal-O bond with oxygen, which alleviates the loss of lattice oxygen and the occurrence of phase change. By adding a dopant containing the above two cations when grinding and mixing the precursor / lithium salt, a one-step method is achieved to improve the cycle performance and rate performance of the positive electrode material in a simple and efficient manner. The applicable object of the present invention is a high-temperature solid-phase reaction system of a transition metal precursor and a lithium salt, and has nothing to do with the type of transition metal precursor. Below we select a commercial transition metal precursor as a representative for discussion.

[0027] Comparative Example 1

[0028] Aluminum-doped lithium-rich manganese-based positive electrode material is prepared by the following steps:

[0029] (1) Li-rich manganese-based commercial precursor (Mn 0.54 Co 0.13 Ni 0.13CO3, 1g), lithium carbonate (Li2CO3), aluminum hydroxide (Al(OH)3) are ground until they are evenly mixed. The materials are divided into three parts according to the molar ratio of aluminum ions to lithium ions of 1%, 3%, and 5%, which correspond to 0.446g lithium carbonate and 0.0089g aluminum hydroxide; 0.437g lithium carbonate and 0.0268g aluminum hydroxide; 0.428g lithium carbonate and 0.0446g aluminum hydroxide respectively.

[0030] (2) The precursor mixture is calcined by a two-step method to obtain a lithium-rich manganese-based positive electrode material, that is, the temperature is increased to 500±20°C at a heating rate of 5°C / min and the temperature is kept for calcination for 6 hours, and then the temperature is increased to 850±20°C at the same heating rate and the temperature is kept for calcination for 14 hours, and the temperature is cooled to room temperature at a cooling rate of 5°C / min to obtain an aluminum-doped lithium-rich manganese-based positive electrode material. According to the molar ratio of aluminum ions to lithium ions in step (1), 1%, 3%, and 5%, the products are named LMR-Al1, LMR-Al3, and LMR-Al5, respectively.

[0031] Comparative Example 2

[0032] Potassium-doped lithium-rich manganese-based positive electrode material is prepared by the following steps:

[0033] (1) Li-rich manganese-based commercial precursor (Mn 0.54 Co 0.13 Ni 0.13 CO3, 1g), lithium carbonate (Li2CO3), and aluminum hydroxide (KOH) are ground until they are evenly mixed. The materials are divided into three parts according to the molar ratio of potassium ions to lithium ions of 1%, 3%, and 5%, which correspond to 0.446g lithium carbonate and 0.0064g aluminum hydroxide; 0.437g lithium carbonate and 0.0192g aluminum hydroxide; 0.428g lithium carbonate and 0.0320g aluminum hydroxide. ;

[0034] (2) The precursor mixture is calcined by a two-step method to obtain a lithium-rich manganese-based positive electrode material, that is, the temperature is increased to 500±20°C at a heating rate of 5°C / min and kept at a temperature for 6 hours, and then the temperature is increased to 850±20°C at the same heating rate and kept at a temperature for 14 hours, and then the temperature is cooled to room temperature at a cooling rate of 5°C / min to obtain a potassium-doped lithium-rich manganese-based positive electrode material. According to the molar ratio of potassium ions to lithium ions in step (1), 1%, 3%, and 5%, the products are named LMR-K1, LMR-K3, and LMR-K5, respectively.

[0035] Comparative Example 3

[0036] The original lithium-rich manganese-based positive electrode material is prepared by the following steps:

[0037] (1) Commercial lithium-rich manganese-based cathode material precursor (Mn 0.54 Co 0.13 Ni0.13 CO3 (1 g) and lithium carbonate (0.45 g) were mixed and ground evenly;

[0038] (2) The precursor mixture is calcined to obtain a lithium-rich manganese-based positive electrode material, that is, the temperature is raised to 500±20°C at a heating rate of 5°C / min and the temperature is kept for calcination for 6 hours, and then the temperature is raised to 850±20°C at the same heating rate and the temperature is kept for calcination for 14 hours, and the temperature is cooled to room temperature at a cooling rate of 5°C / min to obtain a lithium-rich manganese-based positive electrode material (Li 1.2 Mn 0.54 Co 0.13 Ni 0.13 O2), referred to as LMO.

[0039] Figure 1 This is the performance diagram of LMO, LMO-Al1, LMO-Al3, and LMO-Al5 at 1C for 100 cycles. Figure 1 As shown in the figure, the capacity retention rates of LMO, LMO-Al1, LMO-Al3 and LMO-Al5 after 100 cycles at 1C are 75.73%, 85.09%, 88.25% and 84.6%, respectively. This shows that aluminum doping has a significant improvement on the cycle performance of the positive electrode material, among which 3% aluminum doping has the best effect on improving the cycle performance.

[0040] Figure 2 This is a schematic diagram of the discharge median voltage of LMO, LMO-Al1, LMO-Al3, and LMO-Al5 after 100 cycles of 1C. After 100 cycles, the discharge median voltage drops of LMO, LMO-Al1, LMO-Al3, and LMO-Al5 are 0.396V, 0.3339V, 0.2004V, and 0.2135V, respectively, which shows that aluminum doping effectively suppresses the voltage drop during the cycle of the positive electrode material, and 3% aluminum doping still has the best effect in suppressing the voltage drop.

[0041] It can be seen that aluminum doping has a significant effect on the cycle performance of the positive electrode material and the suppression of voltage drop, and the improvement effect is best when the doping amount is 3%.

[0042] Figure 3 The XPS graphs are of LMO in Comparative Example 3 and LMO-Al3 in Comparative Example 1. In order to explore the reason why 3% aluminum doping improves the cycle performance of lithium-rich manganese-based positive electrode materials, XPS tests were performed on the surfaces of the two samples. Figure 3 (a) and (b) show the XPS spectra of Ni 2p and Co 2p at the surface interface of the above two samples, from which it can be seen that the effect of aluminum doping on the chemical valence state of Ni and Co at the surface interface of the positive electrode material is negligible. Figure 3(c) shows the XPS spectra of Mn2p on the surface of LMO and LMO-Al3. After fitting calculation, the average valence of Mn on the surface of LMO and LMO-Al3 is 3.643 and 3.665, respectively, which shows that aluminum doping helps to improve the average valence of Mn on the surface of the positive electrode material. Figure 3 (d) shows the O1s spectra of LMO and LMO-Al3. Figure 3 As shown in the figure, after fitting calculation, the relative content of lattice oxygen on the surface of the original sample is 56.99%, while the relative content of lattice oxygen on the surface of the aluminum-doped sample is 63.79%. The higher the relative content of lattice oxygen on the surface of the sample means the stronger the structural stability of the positive electrode material, which explains why aluminum doping improves the cycle performance of the positive electrode material.

[0043] Figure 4 This is the rate performance diagram of LMO, LMO-K1, LMO-K3, and LMO-K5. Figure 4 As shown in the figure, as the rate increases, the potassium-doped samples show higher and higher discharge specific capacities than the original samples, among which the rate performance improvement effect is most obvious at 3% potassium doping. At 10C, LMO-K3 shows a discharge specific capacity of 111.3 mAh / g, while LMO only shows a discharge specific capacity of 62.8111.3 mAh / g.

[0044] It can be seen that potassium doping has a significant effect on improving the rate performance of positive electrode materials, and the improvement effect is most obvious when the doping amount is 3%.

[0045] Figure 5 The XPS graphs are those of LMO in comparative example 1 and LMO-K3 in comparative example 3. In order to explore the reason why potassium doping improves the rate performance of the positive electrode material on the lithium-rich manganese-based positive electrode material, XPS tests were performed on the surfaces of the two samples. Figure 5 (a) and (b) show the XPS spectra of Ni 2p and Co 2p of LMO and LMO-K3, respectively. As shown in the figure, potassium doping has almost no effect on the oxidation state of Ni and Co on the surface of the positive electrode material. Figure 5 (c) shows the XPS spectra of Mn 2p on the surface of the above two samples. After fitting calculation, the average valence of Mn on the surface of LMO and LMO-K3 is 3.643 and 3.637 respectively, indicating that potassium doping leads to a decrease in the average valence of Mn on the positive electrode material. Figure 5 (d) shows the O1s spectra of LMO and LMO-K3. Figure 5As shown in the figure, after fitting calculation, the relative content of lattice oxygen on the surface of the original sample is 56.99%, while the relative content of lattice oxygen on the surface of the 3% potassium-doped sample is 51.59%, which shows that potassium doping has the function of reducing lattice oxygen and increasing surface oxygen vacancies. More oxygen vacancy concentration on the surface of the positive electrode material helps to improve the rate performance of the positive electrode material, which may be the reason why potassium doping improves the rate performance of the positive electrode material.

[0046] Therefore, aluminum doping can significantly improve the cycle performance of the positive electrode material, and potassium doping can significantly improve the rate performance of the positive electrode material. The improvement effect of single doping of both elements is best when the doping amount is 3%, so in the examples listed below, the total doping amount is controlled to be 3% when aluminum + potassium co-doping is performed for comparison.

[0047] Example

[0048] Aluminum + potassium co-doped lithium-rich manganese-based positive electrode material is prepared by the following steps:

[0049] (1) Li-rich manganese-based commercial precursor (Mn 0.54 Co 0.13 Ni 0.13 CO3, 1g), lithium carbonate (Li2CO3, 0.4387g), aluminum hydroxide (KOH, 0.0094g), aluminum hydroxide (Al(OH)3, 0.013g) are ground until they are uniformly mixed, wherein the aluminum doping and potassium doping are controlled to account for 3% of the molar ratio of lithium ions;

[0050] (2) The precursor mixture was calcined by a two-step method to obtain a lithium-rich manganese-based positive electrode material, that is, the temperature was raised to 500±20°C at a heating rate of 5°C / min and kept at this temperature for 6 hours, and then the temperature was raised to 850±20°C at the same heating rate and kept at this temperature for 14 hours, and then the temperature was lowered to room temperature at a cooling rate of 5°C / min to obtain a 1.5% aluminum + 1.5% potassium co-doped lithium-rich manganese-based positive electrode material (Li 1.165 K 0.0175 Al 0.0175 Mn 0.54 Co 0.13 Ni 0.13 O2), referred to as LMO-Al+K.

[0051] Figure 6 This is the performance diagram of LMO, LMO-Al3, LMO-K3, and LMO-Al+K at 1C for 100 cycles. Figure 6As shown in the figure, after calculation, the capacity retention rates of LMO, LMO-Al3, LMO-K3, and LMO-Al+K after 100 cycles at 1C are 75.73%, 88.25%, 78.36%, and 82.23%, respectively. According to the comparison of the cycle performance of each sample, aluminum doping has a significant effect in improving the cycle performance of the positive electrode material, and the double-doped sample inherits the effect of aluminum doping on improving the cycle performance.

[0052] Figure 7 These are the XRD spectra of LMO, LMO-Al3, LMO-K3, and LMO-Al+K. Figure 7 As shown in the figure, compared with the original sample (LMO), the diffraction peaks of the single-doped and double-doped samples shift to the left, and the left shift of the potassium-doped sample is more obvious, which is attributed to the K + The radius is large, and after being doped into the lithium site, the lithium ion diffusion channel is effectively opened, which means that potassium doping is effective in improving lithium ion diffusion. Figure 8 This is the rate performance diagram of LMO, LMO-Al3, LMO-K3, and LMO-Al+K. Figure 8 As shown in the figure, with the increase of current density, the discharge specific capacity of the potassium-doped samples (LMO-K3, LMO-Al+K) is significantly improved compared with the original sample and the aluminum single-doped sample, which shows that the aluminum + potassium dual-doping inherits the effect of potassium doping in improving the rate performance.

[0053] In summary, the present invention simply and efficiently improves the electrochemical properties of electrode materials through the synergistic effect of aluminum / potassium co-doping. The co-doping strategy takes into account the modification advantages of the two doping elements and achieves the simultaneous improvement of the cycle performance and rate performance of lithium-rich manganese-based positive electrode materials.

Claims

1. A method for improving the performance of electrode materials by co-doping aluminum and potassium, characterized in that: The following steps are involved: (1) Mix and grind the lithium-rich manganese-based cathode material precursor, lithium carbonate, potassium hydroxide and aluminum hydroxide evenly; (2) The obtained precursor mixture is first calcined at 500±20°C for 6 hours and then heated to 850±20°C for 14 hours to obtain a lithium-rich manganese-based positive electrode material.

2. The method according to claim 1, characterized in that The precursor of lithium-rich manganese-based cathode material is Mn 0.54 Co 0.13 Ni 0.13 CO3.

3. The method according to claim 1, characterized in that The mass ratio of lithium-rich manganese-based positive electrode material precursor to lithium carbonate is 1:0.4387.

4. The method according to claim 1, characterized in that The molar ratio of potassium hydroxide to lithium carbonate is 3%, that is, n(K): n(Li)=1.5%.

5. The method according to claim 1, characterized in that The molar ratio of aluminum hydroxide to lithium carbonate is 3%, that is, n(Al):n(Li)=1.5%.

6. The method according to claim 1, characterized in that The heating rate and cooling rate were both 5°C / min.

Citation Information

Cited By

  • Lithium manganate positive electrode material and preparation method thereof, positive electrode plate and battery

    CN121484055A