Black laser radar window glass

By adding cadmium selenide and cadmium telluride to borosilicate glass, and using the light absorption characteristics of CdSe and CdTe, combined with the adjustment of CdO, the high transmittance and insufficient mechanical properties of lidar window glass in the visible light area are solved. Problem, the separation of low transmittance in the visible light area and high transmittance in the near infrared area in the lidar window glass is achieved, and the mechanical and optical properties of the glass are improved.

CN119059735AActive Publication Date: 2024-12-03CNBM RESEARCH INSTITUTE FOR ADVANCED GLASS MATERIALS GROUP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411261762.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-03
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The existing lidar window glass has high transmittance in the visible light area and insufficient mechanical properties. It is difficult to achieve separation of low transmittance in the visible light area and high transmittance in the near infrared area while maintaining the excellent performance of borosilicate glass. During the process, there are problems such as unstable dissolution of the colorant and long melting time at high temperatures.

Method used

Cadmium selenide and cadmium telluride were added to borosilicate glass as colorants, and the light absorption characteristics of the glass were adjusted by controlling the ratio of CdSe and CdTe and the introduction of CdO, and combined with high-temperature and low-pressure melting and annealing treatment, the glass was prepared. Black lidar window glass with extremely low transmittance in the visible light area and high transmittance in the near infrared area.

Benefits of technology

The separation of low transmittance in the visible light area and high transmittance in the near-infrared area is achieved, which improves the mechanical and optical properties of the glass, while shortens the melting time and reduces environmental pollution. It has important lidar window glass applications value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059735A_ABST
    Figure CN119059735A_ABST
Patent Text Reader

Abstract

The invention discloses black laser radar window glass, and belongs to the technical field of glass. The cadmium oxide glass is prepared from a glass colorant, cadmium oxide and a dry base glass batch according to a mass ratio of (0.01-2): (0-10): 100. The window glass prepared by the invention is borosilicate glass, and has very high transmittance in a near-infrared region; the glass coloring agent is obtained by mixing cadmium selenide and cadmium telluride according to the weight percentage of (0-80%): (30-90%), so that the glass has extremely low transmittance in a visible light region, the glass is melted under the negative pressure condition, the volatilization and oxidation of the coloring agent are reduced, and the melting and clarifying quality of the window glass is improved; by adding cadmium oxide, the founding quality and the optical performance of the glass are ensured; therefore, the window glass prepared by the invention is low in transmittance in a visible region, high in transmittance in a near-infrared region, black, environment-friendly and excellent in founding quality and optical performance, and has an important application value in the technical field of laser radar window glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of glass, and in particular, relates to a black laser radar window glass. Background Art

[0002] Laser radar is a radar system that emits laser beams to detect the position, speed and other characteristic quantities of the target. At present, it has been widely used in many fields such as aerospace, national defense, automotive radar, energy, etc. Driven by the rapid development of unmanned driving technology in the 21st century, the development of laser radar equipment has attracted much attention. The optical glass in the laser radar components includes lenses, reflectors, narrow-band filters, window glass, etc. Among them, the laser radar flat window (Laser Flat Windows) is a parallel plane plate that protects electronic sensors or detectors. For confidentiality and security, this window glass is required to have extremely low light wave transmittance in the visible light range, and at the same time have a high transmittance in the near-infrared region, and visually appear black. Optical windows made of materials such as quartz glass or polycarbonate are commonly used on the market. However, these materials have high transmittance in the visible light region, cannot play the role of keeping the internal devices confidential, and some have poor mechanical properties. In view of the above shortcomings, we are waiting to develop a material with extremely low transmittance in the visible light region, high transmittance in the near-infrared region, and good mechanical properties as a window material for laser radar.

[0003] Borosilicate glass has excellent thermal stability, chemical stability, mechanical properties, processability and optical properties. Its excellent properties can be used as lidar window glass in many fields. However, borosilicate glass has high transmittance in the visible light region and near-infrared region. Therefore, it is urgent to find a compound that can affect the optical absorption of borosilicate glass while maintaining other excellent properties of borosilicate glass, so that it has extremely low transmittance in the visible light region without affecting the high transmittance in the near-infrared region.

[0004] Cadmium selenide and cadmium telluride belong to the II-VI group of compounds, which are semiconducting, have large lattice constants, narrow bandgap widths, and obvious intrinsic absorption in the near-infrared region. They are added as colorants to borosilicate glass to develop a laser radar window glass that has strong absorption in the visible light region and high transmittance in the near-infrared region. However, during the preparation process, the melting temperature of borosilicate glass is high, the viscosity is high, and the clarification time is long. In addition, cadmium telluride tends to exist in the glass in a free state during the dissolution process. Free tellurium has strong absorption in the near-infrared region. Therefore, the above problems need to be solved to meet the higher demands in the field of laser radar window glass technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a black laser radar window glass.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A black laser radar window glass is prepared by the following steps:

[0008] S1. Mix the glass colorant with cadmium oxide and dry-base glass batch material, pour into a crucible, and then place in a high-temperature furnace, heat the high-temperature furnace to 1500-1700° C. to melt and clarify to obtain glass liquid;

[0009] S2. Pour the melted glass in step S1 into a mold for molding; place the molded glass in an annealing furnace for annealing at 700-850° C., cut, grind and polish after annealing to obtain black laser radar window glass.

[0010] Furthermore, the mass ratio of the glass colorant, cadmium oxide and dry-base glass batch material is 0.01-2:0-10:100.

[0011] Furthermore, the glass colorant is obtained by mixing cadmium selenide and cadmium telluride in a weight percentage of 0-80%:30-90%.

[0012] Furthermore, the components of the dry-based glass batch in percentage by mass are: SiO2: 70-88%, B2O3: 4-12%, Al2O3: 1-4%, Na2O: 1-4%, K2O: 0.05-0.2%, NaCl: 1-5%, ZnO: 0-5%.

[0013] Furthermore, the dry-based glass batch materials are all chemically pure, wherein the raw material of B2O3 is H3BO3, the raw material of K2O is K2CO3, and the raw material of Na2O is NaNO3.

[0014] Furthermore, the SiO2 in the dry-based glass batch is silicon dioxide aerogel.

[0015] Furthermore, the crucible is a high-purity quartz crucible.

[0016] Furthermore, the high-temperature melting furnace can adjust the gas pressure in the furnace. During clarification, the working gas pressure in the furnace is 0.3-0.7 standard atmospheric pressure, and the melting time is 1-3 hours.

[0017] Furthermore, the annealing furnace is a medium-low temperature muffle furnace, and the annealing time is 0.5-2 hours.

[0018] Borosilicate glass has high transmittance in the visible light region and near infrared region. The glass colorant of the present invention does not contain arsenic and antimony, is environmentally friendly, and is simple and easy to operate. CdSe and CdTe have obvious absorption limits between the visible light and near infrared regions. The present invention utilizes the intrinsic absorption of CdSe and CdTe, adds CdSe and CdTe as colorants in a certain proportion to the borosilicate glass batch material for melting, and obtains borosilicate glass containing CdSe-CdTe. The light absorption is due to the light-excited anions (O 2- 、Se 2- 、TeTe 2- ) to an excited state. 2- 、Te 2- The electrophilic potential is less than O 2- , so less energy can be excited, so that its absorption limit enters the visible light region, so that the glass has extremely low transmittance in the visible light region and is colored. The absorption limit of CdSe-CdTe in glass is generally 710-840nm, and the position of the absorption limit mainly depends on the ratio of CdSe and CdTe. The reaction is complicated during the glass melting heat treatment process. Compared with Se, Te presents a stronger metallic property, has a higher boiling point and a lower vapor pressure. CdTe is easy to present in a free state in the dissolution process and exists in the glass. The free Te has a strong absorption to the near-infrared region. The larger the CdTe content, the more free it is, and the stronger the absorption. For this reason, the present invention adds CdO in the melting composition. When CdO is introduced into the glass, Cd ions can be linked with O ions and are outside the glass network body. During heat treatment, Cd outside the glass network body may be combined with free Te to form CdTe, and free Te is gradually reduced and eliminated, which greatly improves the transmittance of the glass near-infrared region after the introduction of CdO. At the same time, high borosilicate glass has high viscosity and is difficult to remove bubbles, so the melting and clarification time is relatively long, but the long-term high temperature state will also aggravate the generation of free Te. In order to shorten the clarification time and obtain high-quality glass, the present invention adopts a reduced pressure clarification method to accelerate the bubble removal process of the molten glass, improve the glass clarification quality, and shorten the melting and clarification time to achieve better optical properties.

[0019] Beneficial effects of the present invention:

[0020] 1. The window glass prepared by the present invention is borosilicate glass, which has high transmittance in the near-infrared region;

[0021] 2. Glass colorants contain cadmium selenide and cadmium telluride, which can make the glass have extremely low transmittance in the visible light region, thus turning it black;

[0022] 3. High-temperature melting under negative pressure reduces the volatilization and oxidation of colorants during the entire melting process, improves the melting and clarification quality of the black laser radar window glass, and is environmentally friendly;

[0023] 4. The addition of cadmium oxide ensures the melting quality and optical properties of the glass;

[0024] Therefore, the window glass produced by the present invention has low transmittance in the visible light region, high transmittance in the near-infrared region, is black in color, is environmentally friendly, has excellent melting quality and optical properties, and has important application value in the field of laser radar window glass technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described below in conjunction with the accompanying drawings.

[0026] Figure 1 It is a transmittance curve diagram of Examples 1-6 of the present invention.

[0027] Figure 2 Graph showing transmittance of Examples 7-12 of the present invention. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In the embodiments of the present invention, the raw materials of cadmium telluride and cadmium selenide are commercially available CdTe and CdSe compounds prepared by thermal synthesis or deposition method.

[0030] A black laser radar window glass is prepared by the following steps:

[0031] S1. Mix the glass colorant with cadmium oxide and dry-base glass batch material, pour into a high-purity quartz crucible, and then place in a high-temperature furnace, heat the high-temperature furnace to 1500-1700° C. to melt and clarify, and obtain glass liquid;

[0032] S2, pouring the melted glass in step S1 into a mold for molding; placing the molded glass in an annealing furnace for annealing at 700-850° C., cutting, grinding and polishing after annealing to obtain a black laser radar window glass;

[0033] The mass ratio of the glass colorant, cadmium oxide and dry-base glass batch material is 0.01-2:0-10:100;

[0034] The glass colorant is obtained by mixing cadmium selenide and cadmium telluride in weight percentages of 0-80%:30-90%;

[0035] The components of the dry-based glass batch materials in mass percentage are: SiO2: 70-88%, B2O3: 4-12%, Al2O3: 1-4%, Na2O: 1-4%, K2O: 0.05-0.2%, NaCl: 1-5%, ZnO: 0-5%; the dry-based glass batch materials are all chemically pure, wherein the raw material of B2O3 is H3BO3, the raw material of K2O is K2CO3, and the raw material of Na2O is NaNO3; SiO2 is silicon dioxide aerogel.

[0036] By following the above steps and controlling the amount and conditions of the raw materials, Examples 1-12 were obtained, and their properties were measured. The transmittance of Examples 1-12 at wavelengths greater than 600 nm was plotted, which are: Figure 1 and Figure 2 , and then draw the tables as Table 1 and Table 2;

[0037] Table 1

[0038]

[0039]

[0040] Table 2

[0041]

[0042]

[0043] As can be seen from Table 1, in Examples 1-3, the ratio of CdSe to CdTe and the introduction of CdO will affect the transmittance of the glass samples in the visible light region and the near-infrared light region. As the amount of CdTe increases, the glass gradually absorbs more visible light and near-infrared light. The light absorption of the glass is basically the superposition of the light absorption of the above-mentioned CdSe-containing glass and CdTe-containing glass, and neither shows the intrinsic absorption that the CdSe-CdTe solid solution should have;

[0044] In Examples 4-6, as the CdO content increases, the near-infrared transmittance of the glass increases rapidly, and the transmittance in the visible light region decreases sharply. However, after increasing to a certain extent, the absorption in the visible light region remains unchanged, and the transmittance in the near-infrared region decreases. The absorption limit is between 710nm and 840nm. The position of the absorption limit depends on the ratio of CdSe to CdTe, and Figure 1 It can be clearly seen that the ratio of CdSe and CdTe affects the transmittance.

[0045] As can be seen from Table 2, in Examples 7-9, as the high-temperature furnace pressure decreases, the molten glass debubbling time is shortened, which reduces the probability of CdTe producing free Te due to long-term high temperature, and is more conducive to the transmission of light waves in the near-infrared region;

[0046] In Examples 10-12, during the heat treatment process, CdSe-CdTe solid solution microcrystals gradually precipitate in the glass. As the annealing temperature and time increase, the relative amount of CdTe in the solid solution increases, the lattice constant gradually increases, and the bandgap narrows, so that the light absorption limit moves to the long wave, and has different degrees of influence on the visible light region and the near infrared region. Figure 2 It can be clearly seen that by controlling the ratio of CdSe and CdTe and adding appropriate CdO, the transmittance in the infrared light region is better.

[0047] It can be seen from the above two tables that when the amount of CdSe, CdTe and CdO added in the embodiment of the present invention is greater than or equal to 4g, the average transmittance T in the visible light band including but not limited to the range of 380-780nm is less than 5%; the near-infrared band including but not limited to 905nm and 1550nm, the transmittance T≥85%, and the number of visible bubbles (>0.1mm) per square meter of the obtained black laser radar window glass sample is not more than 1. Therefore, the window glass prepared by the present invention has low transmittance in the visible light region, high transmittance in the near-infrared region, black color, and is environmentally friendly, with excellent melting quality and optical properties, and has important application value in the field of laser radar window glass technology.

[0048] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0049] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A black laser radar window glass, characterized in that: Prepared by the following steps: S1. Mix the glass colorant with cadmium oxide and dry-base glass batch material, pour into a crucible, and then place in a high-temperature furnace, heat the high-temperature furnace to 1500-1700° C. to melt and clarify to obtain glass liquid; S2. Pour the melted glass in step S1 into a mold for molding; place the molded glass in an annealing furnace for annealing at 700-850° C., cut, grind and polish after annealing to obtain black laser radar window glass.

2. The black laser radar window glass according to claim 1, characterized in that: The mass ratio of the glass colorant, cadmium oxide and dry-base glass batch material is 0.01-2:0-10:

100.

3. The black laser radar window glass according to claim 1, characterized in that: The glass colorant is obtained by mixing cadmium selenide and cadmium telluride in weight percentages of 0-80%:30-90%.

4. The black laser radar window glass according to claim 1, characterized in that: The components of the dry-based glass batch material in percentage by mass are: SiO2: 70-88%, B2O3: 4-12%, Al2O3: 1-4%, Na2O: 1-4%, K2O: 0.05-0.2%, NaCl: 1-5%, and ZnO: 0-5%.

5. The black laser radar window glass according to claim 4, characterized in that: The dry-base glass batch materials are all chemically pure, wherein the raw material of B2O3 is H3BO3, the raw material of K2O is K2CO3, and the raw material of Na2O is NaNO3.

6. The black laser radar window glass according to claim 4, characterized in that: The SiO2 in the dry-based glass batch material is silicon dioxide aerogel.

7. The black laser radar window glass according to claim 1, characterized in that: The crucible is a high-purity quartz crucible.

8. The black laser radar window glass according to claim 1, characterized in that: The high-temperature melting furnace can adjust the gas pressure in the furnace. During clarification, the working gas pressure in the furnace is 0.3-0.7 standard atmospheric pressure, and the melting time is 1-3 hours.

9. The black laser radar window glass according to claim 1, characterized in that: The annealing furnace is a medium-low temperature muffle furnace, and the annealing time is 0.5-2 hours.

Citation Information

Patent Citations

  • Substrate for an optical filter and optical filter

    CN109809689A

  • Anti-blue-light high-strength aluminosilicate glass and preparation method thereof

    CN110937803A

  • Laser radar window glass clarifying method

    CN117510063A

  • Color optical glass and its use and optical sharp cutoff filter

    CN1406895A

  • New type near infrared prevention glass

    CN1618758A