Cement adhesive as well as preparation method and application thereof

The cement adhesive formulation with aluminate cement, porcelain sand, titanium oxide, and silica powder, along with specific admixtures, addresses the issue of poor cold resistance by forming stress-absorbing bubbles, enhancing mechanical properties and frost resistance in high-altitude cold regions.

CN119059783AActive Publication Date: 2024-12-03NEI MENG GU CHAO GAO YA GONG DIAN JU
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411569803.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-03
Estimated Expiration
2044-11-06

AI Technical Summary

Technical Problem

Existing cement binders used in high-altitude cold regions suffer from poor cold resistance, leading to cracking and failure due to temperature fluctuations.

Method used

A cement adhesive comprising aluminate cement, artificial porcelain sand, titanium oxide, silica powder, and specific admixtures, including an air-entraining agent, water reducer, antifreeze agent, and reinforcing agent, with a controlled water-cement ratio, to enhance cold resistance by forming bubbles that absorb frost heave stress and prevent cracking.

Benefits of technology

The cement adhesive significantly improves cold resistance, maintaining strength and workability while reducing crack formation and shrinkage, as demonstrated by increased compressive and flexural strengths and improved frost resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059783A_ABST
    Figure CN119059783A_ABST
Patent Text Reader

Abstract

The invention provides a cement adhesive as well as a preparation method and application thereof, and belongs to the technical field of cement adhesives. The cement adhesive provided by the invention comprises the following components: aluminate cement, artificial porcelain sand, titanium oxide, silica powder, an additive and water, the water cement ratio of the cement adhesive is 0.1 to 0.2; the admixture comprises an air entraining agent, a water reducing agent, an anti-freezing agent, a reinforcing agent and a steep wave performance improving agent; the water reducing agent is an efficient polycarboxylic acid water reducing agent; the mass of the reinforcing agent is 0.1-0.3% of the total mass of the aluminate cement, the artificial porcelain sand, the titanium oxide and the silica powder. When the air entraining agent is used in a cold region, bubbles formed by the air entraining agent can absorb frost heaving stress, and the damage degree of a cement adhesive is reduced; the bubbles can also reduce the formation of pores and cracks; in the drying process, the bubbles can absorb a part of stress when the cement adhesive shrinks, so that the cold resistance is improved; the water consumption can be controlled by limiting the water-cement ratio, and the cold resistance is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of cement adhesives, and in particular relates to a cement adhesive and a preparation method and application thereof. Background Art

[0002] In high-altitude cold regions, extremely low temperatures can adversely affect the performance of porcelain insulator cement bonds. Improving the quality of cement bonds can enhance their cold resistance, ensuring good adhesion and durability even in extreme low-temperature conditions. This prevents cracking, failure, or degradation of the bond caused by temperature fluctuations, thereby ensuring the proper operation and reliability of insulators.

[0003] Current cement binders primarily consist of aluminate cement, artificial porcelain sand, halloysite, titanium oxide, and admixtures. However, they exhibit poor cold resistance. Temperature fluctuations can cause the cement binder to crack or flake when used in cold regions. Therefore, improving cement binders to enhance their cold resistance has become a pressing technical challenge in this field. Summary of the Invention

[0004] The purpose of the present invention is to provide a cement adhesive and its preparation method and application. The cement adhesive provided by the present invention can improve the cold resistance of the cement adhesive.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The present invention provides a cement adhesive, comprising the following components: aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water; The water-cement ratio of the cement adhesive is 0.1-0.2; The external admixtures include air entraining agent, water reducing agent, antifreeze agent, reinforcing agent and steep wave performance improver; The water reducer is a high-efficiency polycarboxylate water reducer; The mass of the reinforcing agent is 0.1-0.3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0006] Preferably, the mass of the aluminate cement is 45-60% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0007] Preferably, the mass of the artificial porcelain sand is 35-50% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0008] Preferably, the mass of the titanium oxide is 1-3% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0009] Preferably, the particle size of the titanium oxide is 20-80 nm.

[0010] Preferably, the mass of the air-entraining agent is 0.005-0.01% of the mass of the aluminate cement.

[0011] Preferably, the air entraining agent includes at least one of rosin resins, alkyl sulfonic acids, alkyl aromatic sulfonic acids and fatty alcohol sulfonates.

[0012] The present invention also provides a method for preparing the cement adhesive described in the above technical solution, comprising: Aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water are mixed to obtain cement adhesive.

[0013] The present invention also provides the use of the cement adhesive described in the above technical solution or the cement adhesive prepared by the preparation method described in the above technical solution in anti-pollution porcelain insulators in high-altitude and cold areas.

[0014] Preferably, the application includes: pouring cement adhesive into anti-pollution porcelain insulators for high-altitude cold areas, and then sequentially performing steam curing and water curing.

[0015] The present invention provides a cement adhesive, comprising the following components: aluminate cement, artificial porcelain sand, titanium oxide, silica micropowder, an admixture and water; the water-cement ratio of the cement adhesive is 0.1-0.2; the admixture comprises an air entraining agent, a water reducer, an antifreeze agent, a reinforcing agent and a steep wave performance improver; the water reducer is a high-efficiency polycarboxylate water reducer; and the mass of the reinforcing agent is 0.1-0.3% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silica micropowder. The present invention adds an air-entraining agent. In cold regions, the bubbles formed by the air-entraining agent can absorb frost heave stress and reduce damage to the cement adhesive. The bubbles also prevent water penetration, reducing the formation of pores and cracks. Furthermore, during the drying process, the bubbles absorb some of the stress when the cement adhesive shrinks, reducing the degree of shrinkage and the probability of cracking, thereby improving the cold resistance of the cement adhesive. By limiting the range of the water-cement ratio, the amount of water used can be controlled to avoid excessive freezable water in the cement adhesive, which can lead to rapid freezing, poor bubble structure, and excessive average bubble spacing, which can reduce cold resistance. Experimental results show that the cement adhesive provided by the present invention can significantly improve cold resistance while maintaining workability and strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is the compressive strength of the cement adhesives prepared in Example 1 and Comparative Examples 1-2; Figure 2 is the flexural strength of the cement adhesives prepared in Example 1 and Comparative Examples 1-2; Figure 3 is the compressive strength of the cement adhesive prepared in Example 2; Figure 4 is the flexural strength of the cement adhesive prepared in Example 2; Figure 5 is the compressive strength of Application Example 1 and Comparative Application Example 1; Figure 6 is the flexural strength of Application Example 1 and Comparative Application Example 1; Figure 7 The elastic modulus of the cement adhesives prepared in Examples 4 and 5 and Comparative Examples 4 and 5 after 28 days of frost resistance testing. DETAILED DESCRIPTION

[0017] The present invention provides a cement adhesive, comprising the following components: aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water; The water-cement ratio of the cement adhesive is 0.1-0.2; The external admixtures include air entraining agent, water reducing agent, antifreeze agent, reinforcing agent and steep wave performance improver; The water reducer is a high-efficiency polycarboxylate water reducer; The mass of the reinforcing agent is 0.1-0.3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0018] The present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.

[0019] In the present invention, the cement binder comprises aluminate cement. In the present invention, the aluminate cement is a matrix material.

[0020] As an embodiment, the aluminate cement may be CA50-II aluminate cement.

[0021] In the present invention, the cement adhesive further comprises artificial porcelain sand; the particle size of the artificial porcelain sand is preferably 30-80 mesh. In the present invention, the artificial porcelain sand has good wear resistance, corrosion resistance, and high temperature resistance, and can effectively improve the fluidity of the cement adhesive.

[0022] In the present invention, the cement binder also includes titanium oxide; the titanium oxide preferably has a particle size of 20 to 80 nm. In the present invention, the titanium oxide in the cement binder can significantly improve the mechanical properties and cold resistance of the cement binder. The nano-sized titanium oxide can accelerate cement hydration, reduce setting time, and enhance mechanical properties.

[0023] In the present invention, the cement binder further comprises silica powder; the particle size of the silica powder is preferably 0.1 to 0.2 μm; and the SiO2 content in the silica powder is preferably ≥ 90.0 wt%. In the present invention, the silica powder can significantly improve the mechanical properties and cold resistance of the cement binder.

[0024] Based on the total mass of aluminate cement, artificial porcelain sand, titanium oxide, and silica powder as 100%, the mass content of aluminate cement is preferably 45-60%; the mass content of artificial porcelain sand is preferably 35-50%; the mass content of titanium oxide is preferably 1-3%; and the mass content of silica powder is preferably the remainder. Limiting the contents of aluminate cement, artificial porcelain sand, titanium oxide, and silica powder within the aforementioned ranges can further improve the cold resistance of the cement adhesive.

[0025] As an embodiment, based on the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder as 100%, the mass content of the aluminate cement can be 50-55%; the mass content of the artificial porcelain sand can be 43-45%; the mass content of the titanium oxide can be 2%; and the mass content of the silica powder can be 5%.

[0026] In the present invention, the cement adhesive further includes an admixture; the admixture includes an air-entraining agent. In cold regions, the bubbles formed by the air-entraining agent can absorb frost heave stress and reduce damage to the cement adhesive. The bubbles also prevent water penetration, reducing the formation of pores and cracks. Furthermore, during the drying process, the bubbles absorb some of the stress when the cement adhesive shrinks, reducing the degree of shrinkage and the probability of cracks, thereby improving the cold resistance of the cement adhesive.

[0027] In the present invention, the mass of the air-entraining agent is preferably 0.005-0.01% of the mass of the aluminate cement; the air-entraining agent preferably comprises at least one of rosin resins, alkyl sulfonic acids, alkyl aromatic sulfonic acids, and fatty alcohol sulfonates. Limiting the mass of the air-entraining agent to the above range can further improve the cold resistance of the cement adhesive.

[0028] As an embodiment, the mass of the air-entraining agent may be 0.006-0.008% of the mass of the aluminate cement; the air-entraining agent may be AE330 air-entraining agent.

[0029] In the present invention, the external admixture further comprises a water reducing agent, an antifreeze agent, a reinforcing agent and a steep wave performance improving agent.

[0030] In the present invention, the water reducer is a high-efficiency polycarboxylate water reducer; the mass of the water reducer is preferably 0.1-0.3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide, and silica powder. In the present invention, the use of a high-efficiency polycarboxylate water reducer in the preparation of cement adhesive can significantly improve its performance. This water reducer can effectively reduce the porosity in the cement slurry, thereby increasing the density of the slurry, not only improving the strength of the cement adhesive but also enhancing its compressive strength. By using a high-efficiency polycarboxylate water reducer, the overall performance of the cement adhesive can be improved while maintaining construction performance, making it more suitable for various engineering requirements.

[0031] In the present invention, the water reducer is preferably a polycarboxylate water reducer with acrylic acid / methacrylic acid as the backbone or a polycarboxylate water reducer with maleic anhydride as the backbone. The present invention does not specifically limit the source of the water reducer; a high-efficiency polycarboxylate water reducer well known to those skilled in the art can be used.

[0032] As an embodiment, the mass of the water reducer can be 0.1-0.2% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0033] In the present invention, the antifreeze agent is preferably an organic alcohol; the mass of the antifreeze agent is preferably 0.1-0.3% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide, and silica powder. In the present invention, the antifreeze agent can improve the antifreeze effect of the cement adhesive.

[0034] As an embodiment, the mass of the antifreeze agent can be 0.2-0.25% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0035] In the present invention, the reinforcing agent is preferably polypropylene fiber; the diameter of the polypropylene fiber is preferably 0.02-0.04 mm; the length of the polypropylene fiber is preferably 2-3 mm; and the mass of the reinforcing agent is 0.1-0.3% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide, and silica powder. In the present invention, the reinforcing agent has the characteristics of high strength and high modulus, which can effectively improve the flexural properties of the cement adhesive. At the same time, the reinforcing agent can prevent the flexural strength from decreasing with age, thereby ensuring the stability of the cement adhesive at different stages of use. By using polypropylene fiber as a reinforcing agent, the cement adhesive can maintain good performance during long-term use, meeting various engineering requirements.

[0036] As an embodiment, the mass of the reinforcing agent can be 0.2-0.25% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0037] In the present invention, the steep wave performance improver is preferably sodium chloride; the mass of the steep wave performance improver is preferably 0.02-0.05% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide, and silica powder. In the present invention, the steep wave performance improver can improve the steep wave performance of the cement adhesive.

[0038] As an embodiment, the mass of the steep wave performance improver can be 0.03-0.04% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

[0039] In the present invention, the cement adhesive further comprises water. In the present invention, the water is a solvent.

[0040] In the present invention, the water-cement ratio of the cement binder is 0.1-0.2, preferably 0.14-0.19, and more preferably 0.15-0.18. By limiting the range of the water-cement ratio, the amount of water used can be controlled, thus preventing excessive freezable water in the cement binder, which can lead to rapid freezing, poor cell structure, and excessively large average cell spacing, thus reducing cold resistance.

[0041] The present invention adds an air-entraining agent. In cold regions, bubbles formed by the air-entraining agent can absorb frost heave stress and reduce the degree of damage to the cement adhesive. The bubbles can also prevent moisture penetration and reduce the formation of pores and cracks. At the same time, during the drying process, the bubbles can also absorb part of the stress when the cement adhesive shrinks, reduce the degree of shrinkage, reduce the probability of crack occurrence, and thus improve the cold resistance of the cement adhesive. By limiting the range of the water-cement ratio, the amount of water can be controlled, avoiding excessive freezable water content in the cement adhesive, too fast freezing speed, deterioration of the bubble structure, excessively large average bubble spacing, and reduced cold resistance.

[0042] The present invention also provides a method for preparing the cement adhesive described in the above technical solution, comprising: Aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water are mixed to obtain cement adhesive.

[0043] The present invention has no particular limitation on the mixing operation of the aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water, and the technical scheme for preparing the mixed material well known to those skilled in the art can be adopted.

[0044] The preparation method provided by the invention has simple process and is suitable for industrial production.

[0045] The present invention also provides the use of the cement adhesive described in the above technical solution or the cement adhesive prepared by the preparation method described in the above technical solution in anti-pollution porcelain insulators in high-altitude and cold areas.

[0046] In the present invention, the cement adhesive is preferably applied as a buffer layer to the surface of anti-pollution porcelain insulators for use in high-altitude cold regions before application; the material of the buffer layer is preferably asphalt. The thickness of the buffer layer is not particularly limited and can be applied using procedures familiar to those skilled in the art. In the present invention, applying a buffer layer to the surface of anti-pollution porcelain insulators for use in high-altitude cold regions can improve the electrical performance of the cement adhesive.

[0047] In the present invention, the application preferably includes: pouring the cement adhesive into the anti-pollution type porcelain insulator for high-altitude cold areas, and then sequentially performing steam curing and water curing.

[0048] The present invention has no special limitation on the operation of pouring the cement adhesive into the anti-pollution porcelain insulator in high-cold areas, and the operation well known to those skilled in the art can be adopted.

[0049] In the present invention, the steam curing temperature is preferably 45-55°C; the steam curing time is preferably 5-6 hours; the water curing temperature is preferably 20-30°C; and the water curing time is preferably 5-6 hours. The present invention adopts a composite curing mode of sequential steam curing and water curing. In this curing mode, the cement adhesive is first steam-cured to quickly achieve a certain strength; then water curing is performed to ensure the stability of the cement adhesive during later use. This composite curing mode can effectively reduce the decline in the flexural strength of the cement adhesive in the middle and late stages, thereby improving its overall performance.

[0050] As an embodiment, the temperature of the steaming can be 50-55°C; the temperature of the water-curing can be 25-30°C.

[0051] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the embodiments described are only some of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0052] Example 1 The components of cement adhesive are: aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water; The external admixtures are air entraining agent, water reducing agent, antifreeze agent, reinforcing agent and steep wave performance improver; The mass of the aluminate cement is 50% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the model is CA50-II type aluminate cement; The mass of the artificial porcelain sand is 43% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the particle size is 30-80 mesh; The mass of the titanium oxide is 2% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the particle size is 20-80 nm; The mass of the silicon micropowder is 5% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silicon micropowder; the particle size of the silicon micropowder is 0.1-0.2 μm; the content of SiO2 in the silicon micropowder is 98wt%; The mass of the air entraining agent is 0.008% of the mass of the aluminate cement, and the air entraining agent is AE330 air entraining agent; The water reducer is XCA-100 polycarboxylic acid high-performance water reducer; the mass of the water reducer is 0.2% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The antifreeze agent is an organic alcohol, and its mass is 0.1% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The reinforcing agent is polypropylene fiber with a diameter of 0.02-0.04 mm, a length of 2.5 mm, and a mass of 0.2% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The steep wave performance improver is sodium chloride, the mass of which is 0.04% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The water-cement ratio of the cement binder is 0.13; The preparation method of the cement adhesive is: Aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water are mixed to obtain cement adhesive.

[0053] Comparative Example 1 Based on Example 1, titanium oxide was omitted, the mass of the artificial porcelain sand was modified to 45% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, the water-cement ratio was modified to 0.19, and other conditions remained unchanged.

[0054] Comparative Example 2 On the basis of Example 1, the artificial porcelain sand was changed to river sand, the water-cement ratio was changed to 0.14, and other conditions remained unchanged.

[0055] The cement adhesives prepared in Example 1 and Comparative Examples 1-2 were subjected to performance tests after curing in water at 25°C for 5 hours. The flexural strength, compressive strength, and shrinkage tests were conducted in accordance with JB / T 4307-2004 "Cement adhesives for insulator assembly." The fluidity of the cement adhesive was tested in accordance with GB / T 2419-2005 "Determination of fluidity of cement mortar." The results are shown in Tables 1-2. Figure 1 and Figure 2 As shown; Figure 1 is the compressive strength of the cement adhesives prepared in Example 1 and Comparative Examples 1-2, Figure 2Flexural strength of the cement adhesives prepared in Example 1 and Comparative Examples 1-2.

[0056] Table 1 Performance data of cement adhesives prepared in Example 1 and Comparative Examples 1-2

[0057] Table 2 Performance data of cement adhesives prepared in Example 1 and Comparative Examples 1-2

[0058] From Table 1~2, Figure 1 and Figure 2 It can be seen that the flexural strength of the cement adhesive of the present invention can be increased by 14.5 MPa, the compressive strength can be increased by 34 MPa, and the problem of decreased flexural strength of the cement adhesive in the middle and late stages can be significantly improved.

[0059] Example 2 Based on Example 1, the mass content of the reinforcing agent was modified to 0.1%, and other conditions remained unchanged.

[0060] The performance test of the cement adhesive prepared in Example 2 was carried out according to the test method of Example 1 after curing in water at 25°C for 5 hours. The results are shown in Table 3. Figure 3 and Figure 4 As shown, Figure 3 is the compressive strength of the cement adhesive prepared in Example 2, Figure 4 The flexural strength of the cement adhesive prepared in Example 2.

[0061] Table 3 Performance data of cement adhesive prepared in Example 2

[0062] From Table 3, Figure 3 and Figure 4 It can be seen that the present invention can significantly improve the strength of cement adhesive and effectively prevent the flexural strength from decreasing with age.

[0063] Example 3 Based on Example 1, the mass content of the reinforcing agent was modified to 0.3%, and other conditions remained unchanged.

[0064] Application Example 1 The cement adhesive prepared in Example 3 was poured into the anti-pollution porcelain insulator for high-altitude cold areas, and then steam-cured at 48° C. for 3 h and water-cured at 25° C. for 3 h.

[0065] Comparative Example 3 On the basis of Example 3, the type of water reducer was changed to a naphthalene-based water reducer, model SBTJM®-B naphthalene-based high-efficiency water reducer, and other conditions remained unchanged.

[0066] Comparative Application Example 1 The cement adhesive prepared in Comparative Example 3 was poured into anti-pollution porcelain insulators for high-cold areas, and then steam-cured at 48° C. for 3 h and water-cured at 25° C. for 3 h.

[0067] According to the test method of Example 1, performance tests were performed on Example 1 and Comparative Application Example 1. The results are shown in Tables 4 and 5. Figure 5 and Figure 6 As shown, Figure 5 is the compressive strength of Application Example 1 and Comparative Application Example 1, Figure 6 It is the flexural strength of Application Example 1 and Comparative Application Example 1.

[0068] Table 4 Performance data of application example 1 and comparative application example 1

[0069] Table 5 Performance data of application example 1 and comparative application example 1

[0070] From Table 4~5, Figure 5 and Figure 6 It can be seen that the use of high-efficiency polycarboxylate water reducer can greatly improve the mechanical properties of cement adhesive, with the compressive strength increased by up to 44.4 MPa and the flexural strength increased by up to 11.5 MPa.

[0071] Comparative Example 4 Based on Example 1, the air entraining agent was omitted, and the water-cement ratio was changed to 0.2, while other conditions remained unchanged.

[0072] Example 4 Based on Example 1, the water-cement ratio was modified to 0.2, while other conditions remained unchanged.

[0073] Comparative Example 5 Based on Example 1, the air entraining agent was omitted, and the water-cement ratio was modified to 0.15, while other conditions remained unchanged.

[0074] Example 5 Based on Example 1, the water-cement ratio was modified to 0.15, while other conditions remained unchanged.

[0075] The cement adhesives prepared in Examples 1 to 5 and Comparative Examples 4 to 5 were subjected to performance tests after curing in water at 25°C for 6 hours. The frost resistance of the cement adhesives was tested according to the national standard "Test Method for Frost Resistance of Cement Mortar" (GB / T 41060-2021). After the frost resistance test, the frost resistance data of the cement adhesives prepared in Examples 1 to 3 after curing are shown in Table 6. The elastic modulus of the cement adhesives prepared in Examples 4 to 5 and Comparative Examples 4 to 5 after curing for 28 days is shown in Table 6. Figure 7 shown.

[0076] Table 6 Antifreeze performance data of the cement adhesives prepared in Examples 1 to 3 after curing

[0077] It can be seen from Table 6 that the cement adhesive provided by the present invention has excellent frost resistance.

[0078] from Figure 7 It can be seen that by adjusting the water-cement ratio and the amount of air-entraining agent, the cold resistance of the cement adhesive can be significantly improved while ensuring its working performance and strength.

[0079] Example 6 The components of cement adhesive are: aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water; The external admixtures are air entraining agent, water reducing agent, antifreeze agent, reinforcing agent and steep wave performance improver; The mass of the aluminate cement is 60% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the model is CA50-II type aluminate cement; The mass of the artificial porcelain sand is 35% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the particle size is 30-80 mesh; The mass of the titanium oxide is 1% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the particle size is 20-80 nm; The mass of the silicon micropowder is 4% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silicon micropowder; the particle size of the silicon micropowder is 0.1-0.2 μm; the content of SiO2 in the silicon micropowder is 98wt%; The mass of the air entraining agent is 0.01% of the mass of the aluminate cement, and the air entraining agent is AE330 air entraining agent; The water reducer is XCA-100 polycarboxylic acid high-performance water reducer; the mass of the water reducer is 0.3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The antifreeze agent is an organic alcohol, and its mass is 0.2% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The reinforcing agent is polypropylene fiber with a diameter of 0.02-0.04 mm, a length of 2.5 mm, and a mass of 0.1% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The steep wave performance improver is sodium chloride, the mass of which is 0.02% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The water-cement ratio of the cement binder is 0.13; The preparation method of the cement adhesive is: Aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water are mixed to obtain cement adhesive.

[0080] Example 7 The components of cement adhesive are: aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water; The external admixtures are air entraining agent, water reducing agent, antifreeze agent, reinforcing agent and steep wave performance improver; The mass of the aluminate cement is 45% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the model is CA50-II type aluminate cement; The mass of the artificial porcelain sand is 50% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the particle size is 30-80 mesh; The mass of the titanium oxide is 3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder, and the particle size is 20-80 nm; The mass of the silicon micropowder is 2% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silicon micropowder; the particle size of the silicon micropowder is 0.1-0.2 μm; the content of SiO2 in the silicon micropowder is 98wt%; The mass of the air entraining agent is 0.005% of the mass of the aluminate cement, and the air entraining agent is AE330 air entraining agent; The water reducer is XCA-100 polycarboxylic acid high-performance water reducer; the mass of the water reducer is 0.1% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The antifreeze agent is an organic alcohol, and its mass is 0.3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The reinforcing agent is polypropylene fiber with a diameter of 0.02-0.04 mm, a length of 2.5 mm, and a mass of 0.3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The steep wave performance improver is sodium chloride, the mass of which is 0.05% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder; The water-cement ratio of the cement binder is 0.13; The preparation method of the cement adhesive is: Aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water are mixed to obtain cement adhesive.

[0081] The cement adhesives prepared in Examples 6 and 7 were subjected to performance tests according to the test method of Example 1 after curing in water at 25° C. for 5 hours. The results are shown in Tables 7 and 8.

[0082] Table 7 Performance data of cement adhesives prepared in Examples 6-7

[0083] Table 8 Performance data of cement adhesives prepared in Examples 6-7

[0084] It can be seen from Tables 7 and 8 that the cement adhesive of the present invention has excellent mechanical strength.

[0085] The cement adhesives prepared in Examples 6 and 7 were cured in water at 25°C for 6 hours, and then the frost resistance of the cement adhesives was tested according to the national standard "Test Method for Frost Resistance of Cement Mortar" (GB / T 41060-2021). After the frost resistance test, the frost resistance data of the cement adhesives prepared in Examples 6 and 7 after curing are shown in Table 9.

[0086] Table 9 Antifreeze performance data of the cement adhesive prepared in Examples 6-7 after curing

[0087] It can be seen from Table 9 that the cement adhesive provided by the present invention has excellent frost resistance.

[0088] It can be seen from the above embodiments and comparative examples that the cement adhesive provided by the present invention can improve cold resistance.

[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A cement adhesive, characterized in that: The invention comprises the following components: aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water; The water-cement ratio of the cement adhesive is 0.1-0.2; The external admixtures include air entraining agent, water reducing agent, antifreeze agent, reinforcing agent and steep wave performance improving agent; The water reducer is a high-efficiency polycarboxylate water reducer; The mass of the reinforcing agent is 0.1-0.3% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silicon powder.

2. The cement adhesive according to claim 1, characterized in that: The mass of the aluminate cement is 45-60% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

3. The cement adhesive according to claim 1, characterized in that: The mass of the artificial porcelain sand is 35-50% of the total mass of aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

4. The cement adhesive according to claim 1, characterized in that: The mass of the titanium oxide is 1-3% of the total mass of the aluminate cement, artificial porcelain sand, titanium oxide and silica powder.

5. The cement adhesive according to claim 1 or 4, characterized in that: The particle size of the titanium oxide is 20-80 nm.

6. The cement adhesive according to claim 1, characterized in that: The mass of the air entraining agent is 0.005-0.01% of the mass of the aluminate cement.

7. The cement adhesive according to claim 1 or 6, characterized in that: The air entraining agent includes at least one of rosin resins, alkyl sulfonic acids, alkyl aromatic sulfonic acids and fatty alcohol sulfonates.

8. The method for preparing the cement adhesive according to any one of claims 1 to 7, characterized in that: include: Aluminate cement, artificial porcelain sand, titanium oxide, silica powder, admixture and water are mixed to obtain cement adhesive.

9. Use of the cement adhesive according to any one of claims 1 to 7 or the cement adhesive prepared by the preparation method according to claim 8 in anti-pollution porcelain insulators in high-cold areas.

10. The use according to claim 9, characterized in that: The application comprises: pouring cement adhesive into anti-pollution porcelain insulators in high-cold areas, and then sequentially performing steam curing and water curing.

Citation Information

Patent Citations

  • Extremely cold type cement adhesive

    CN107500651A

  • Porcelain insulator with high cold resistance and preparation method thereof

    CN111018485A

  • Cement adhesive as well as preparation method and application thereof

    CN116425479A

  • Cement adhesive for quickly testing strength of porcelain insulator porcelain piece as well as preparation method and application of cement adhesive

    CN117756484A