Composite fluorescent ceramic for laser illumination and preparation method thereof
By engraving the micro-convex lens array structure on the fluorescent ceramic and co-firing it with transparent ceramics, the problem of insufficient heat dissipation ability of the fluorescent ceramics is solved, efficient photon emission and heat transfer are achieved, luminous efficiency is improved, and the yellow ring effect is avoided. for high power laser lighting.
Patent Information
- Application Number
- CN202411209834.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
Fluorescent ceramics lack heat dissipation capabilities under high power density lasers, resulting in reduced luminescence efficiency, increased temperature and yellow ring effect, limiting their application in laser illumination.
The YAG:Ce fluorescent ceramic with a micro-convex lens array structure on the surface is co-fired with YAG transparent ceramics. The photon exit angle and heat transfer are improved through the micro-convex lens array structure, and the exit and heat dissipation capabilities of the pre-light are enhanced to achieve white light output.
It improves luminous efficiency, enhances heat dissipation ability, avoids yellow ring phenomenon, can withstand high power density excitation, and is suitable for high power lighting devices.
Smart Images

Figure CN119059807A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluorescent ceramics, and in particular to a composite fluorescent ceramic for laser lighting and a preparation method thereof. Background Art
[0002] Laser as the excitation source to excite fluorescent ceramics has many advantages such as high brightness, long range, long life and small size. It can be widely used in outdoor square lighting, sports venues, car headlights, aviation and marine lighting. However, fluorescent ceramics are not suitable for high power density lasers (>10W / mm 2 ) under the excitation of the laser, the laser irradiation area of the fluorescent ceramic will gather a lot of heat (the main source is the energy loss in the light conversion process). Since the thermal conductivity of the fluorescent ceramic is about 12Wm -1 K -1 , which is not enough to dissipate the heat quickly, causing the ceramic temperature at the laser point to rise sharply, resulting in a decrease in luminous intensity and luminous saturation. In addition, the refractive index of fluorescent ceramics is relatively high, such as the refractive index of YAG is n = 1.84, so part of the light is limited by total internal reflection inside the material (the refractive index of air is n = 1.0), causing the fluorescence to be confined inside the ceramic, which not only causes a decrease in the luminous efficiency of the material, but also causes uneven mixing of the emitted blue light and yellow light, resulting in a yellow ring effect, affecting the lighting effect.
[0003] At present, in order to achieve higher luminous efficiency and luminous quality, researchers have made special structural designs for fluorescent materials. 3 Al 5 O 12 :Ce Phosphor-in-Glass Film:A New Composite Color Converter for Next-Generation High-Brightness Laser-Driven Lightings.LASER PHOTONICS REV,12(16)2022.) reported that a YAG:Ce PiG glass film was coated on a high thermal conductivity sapphire substrate to reduce the temperature of the laser spot and increase the saturation threshold of the fluorescent material. However, due to the poor thermal transfer ability of glass phosphors, at a high power density of 10.05W / mm 2Under power excitation, the final luminous efficiency is only 135lm / W. In addition, with the increase of laser power, the temperature at the laser spot of the fluorescent ceramic gradually increases, but due to the insufficient heat dissipation capacity of the fluorescent ceramic, thermal quenching will occur, and even the ceramic will be broken due to the excessive temperature at the spot. The trapezoidal double-layer composite fluorescent ceramic disclosed in CN112537953A uses a combination of yellow / green + red ceramics to achieve the output of high-quality light sources, but the composite of the two luminescent ceramics has serious defects and lacks a high thermal conductivity substrate as a heat dissipation, which also limits the high-power output of the composite ceramic. In addition, when using laser lighting, the mixing of blue light and yellow light is not uniform, resulting in the yellow ring phenomenon in the output light source, which is also a major obstacle to limiting the application of laser lighting.
[0004] In order to solve the problem of low heat dissipation capacity of fluorescent ceramics in laser lighting, a second phase can be introduced to improve the thermal conductivity of the ceramic as a whole. However, in the composite ceramic, the second phase with high thermal conductivity not only exists as a dispersed phase in the matrix to reduce the heat dissipation capacity, but also causes excessive absorption of blue light for transmissive laser lighting, resulting in reduced blue light emission and output of yellow light. Secondly, the yellow ring effect still exists in laser lighting, and the output blue and yellow light are mixed unevenly. This can be solved by using Al 2 O 3 The second phase covers and limits the spot area to integrate the yellow and blue light. However, since the two are not made of the same material, there will be problems at the joints, which will affect the luminescence effect of the composite ceramic. Summary of the invention
[0005] One of the purposes of the present invention is to provide a composite fluorescent ceramic for laser lighting, which, as a luminescent material, has the advantages of high heat dissipation capacity, high luminous efficiency, strong front light emission, and no yellow ring phenomenon.
[0006] The second object of the present invention is to provide a method for preparing a composite structure fluorescent ceramic for laser lighting, which is easy to realize industrial production.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] In a first aspect, the present invention provides a composite fluorescent ceramic for laser lighting, wherein the composite fluorescent ceramic is obtained by co-firing a YAG:Ce fluorescent ceramic having a micro-convex lens array structure on the surface and a YAG transparent ceramic, wherein the YAG:Ce fluorescent ceramic is used to improve the emission angle of photons and obtain collimated forward light, and the YAG transparent ceramic is used to collect heat generated by the fluorescent layer and transfer the heat.
[0009] Preferably, the doping concentration of Ce in the YAG:Ce fluorescent ceramic is 0.01-0.2 at %.
[0010] The composite fluorescent ceramic can achieve high-brightness white light emission under the excitation of a blue light LD chip with a wavelength of 455nm and can withstand an excitation power density of 65W / mm 2 ~75W / mm 2 , luminous efficiency 220 ~ 260lm / W, beam divergence angle 90 ° ~ 110 °.
[0011] In a second aspect, the present invention also provides a method for preparing the composite fluorescent ceramic for laser lighting, which specifically comprises the following steps:
[0012] Step 1: Prepare YAG:Ce powder and YAG powder respectively;
[0013] Step 2: dry pressing is used to press the YAG:Ce / YAG composite ceramic green body, and then vacuum sintering and annealing are performed in sequence to obtain the YAG:Ce / YAG composite ceramic;
[0014] Step three: Use laser engraving technology to engrave a micro-convex lens array structure on the YAG:Ce surface of the composite ceramic. The bottom plane circle diameter of the micro-convex lens is 0.2-0.3mm and the height is 0.1-0.15mm, and finally a composite fluorescent ceramic with a thickness of 0.8-1.4mm is obtained.
[0015] Preferably, in step 2, YAG powder is pressed first, and then YAG:Ce powder is pressed; wherein the mass ratio of the two is 1:1.
[0016] Preferably, in step 2, the vacuum sintering temperature is 1740° C. to 1770° C., and the holding time is 10 to 15 hours.
[0017] Preferably, in step 2, the annealing temperature is 1300-1500° C., and the holding time is 8-12 hours.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The composite ceramic prepared by the present invention can achieve high-brightness white light emission under the excitation of a blue light LD chip with a wavelength of 455nm and can withstand an excitation power density of 65W / mm 2 ~75W / mm 2 , luminous efficiency 220 ~ 260lm / W, beam divergence angle 90 ° ~ 110 °.
[0020] (2) The composite fluorescent ceramic in the present invention is composed of a lens array YAG:Ce fluorescent ceramic and a YAG transparent ceramic. The YAG:Ce fluorescent ceramic with a micro-convex lens array structure on the surface can change the emission direction of the internal light path, enhance the emission of the front light, and make the emission directions of blue light and yellow light close to each other, enhance the mixing of yellow and blue light, and realize white light output; secondly, it breaks the total internal reflection effect of internal photons, so that photons are emitted from the light-emitting surface to obtain a higher luminous efficiency; finally, the lens structure increases the contact area between the surface of the fluorescent ceramic and the air, and the heat generated by the fluorescent layer can be transferred to the YAG transparent ceramic and the air in both directions at the same time, further improving the heat dissipation of the ceramic.
[0021] (3) The present invention adopts dry pressing to prepare the composite fluorescent ceramic blank, which can effectively control the fine structure of the blank without defects such as cracks and deformation, and at the same time achieve mass production, which is conducive to the industrialization of the preparation of the composite fluorescent ceramic.
[0022] (4) The present invention adopts a co-firing scheme to tightly bond YAG transparent ceramics and YAG:Ce fluorescent ceramics together. Since both belong to the YAG system and have similar thermal expansion coefficients, they can be sintered in one step without cracking. The highly transparent YAG ceramics provide better heat dissipation, enabling them to be used in high-power lighting devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the composite fluorescent ceramic blank of the present invention; in the figure: 1-YAG:Ce fluorescent ceramic; 2-YAG transparent ceramic;
[0024] Figure 2 This is a light path model diagram of the composite fluorescent ceramic in the present invention;
[0025] Figure 3 This is a graph of the luminous efficiency of the composite fluorescent ceramics prepared in Examples 1-3 of the present invention;
[0026] Figure 4 This is a spatial light intensity distribution diagram of YAG:Ce / YAG prepared in Example 2 of the present invention;
[0027] Figure 5 This is a transmittance diagram of YAG:Ce / YAG prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] The present invention provides a composite fluorescent ceramic for laser lighting, the structure of which is as follows Figure 2As shown, the composite fluorescent ceramic is obtained by co-firing a YAG:Ce fluorescent ceramic 1 having a micro-convex lens array structure on the surface and a YAG transparent ceramic 2. The YAG:Ce fluorescent ceramic 1 is used to improve the emission angle of photons and obtain collimated forward light, and the YAG transparent ceramic 2 is used to collect the heat generated by the fluorescent layer and transfer the heat.
[0029] The YAG:Ce fluorescent ceramic 1 with a micro-convex lens array structure on the surface can change the emission direction of the internal light path, enhance the emission of the front light, and make the emission directions of blue light and yellow light close to each other, enhance the mixing of yellow and blue light, and realize white light output; secondly, it breaks the total internal reflection effect of internal photons, so that photons are emitted from the light-emitting surface to obtain higher luminous efficiency; finally, the lens structure increases the contact area between the surface of the fluorescent ceramic and the air, and the heat generated by the fluorescent layer can be transmitted to the YAG transparent ceramic 2 and the air in both directions at the same time, further improving the heat dissipation of the ceramic.
[0030] In a specific embodiment, the doping concentration of Ce in the YAG:Ce fluorescent ceramic is 0.01-0.2 at%, for example, the doping concentration of Ce is 0.01 at%, 0.05 at%, 0.1 at%, 0.15 at%, or 0.2 at%.
[0031] The present invention also provides a method for preparing the composite fluorescent ceramic for laser lighting, which specifically comprises the following steps:
[0032] Step 1: Prepare YAG:Ce powder and YAG powder respectively;
[0033] Step 2: Dry pressing to form YAG:Ce / YAG composite ceramic blank (blank structure as shown in Figure 1 As shown, the YAG:Ce fluorescent ceramic 1 is on the top and the YAG transparent ceramic 2 is on the bottom), and then vacuum sintering and annealing are performed in sequence to obtain a YAG:Ce / YAG composite ceramic;
[0034] Step three: Use laser engraving technology to engrave a micro-convex lens array structure on the YAG:Ce surface of the composite ceramic. The bottom plane circle diameter of the micro-convex lens is 0.2-0.3mm and the height is 0.1-0.15mm, and finally a composite fluorescent ceramic with a thickness of 0.8-1.4mm is obtained.
[0035] In a specific embodiment, in step 2, YAG powder is pressed first, and then YAG:Ce powder is pressed; wherein the mass ratio of the two is 1:1.
[0036] In a specific embodiment, in step 2, the vacuum sintering temperature is 1740°C to 1770°C, and the insulation time is 10 to 15 hours; for example, the vacuum sintering temperature is 1740°C, 1750°C, 1760°C, and 1770°C, and the insulation time is 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, and 15 hours.
[0037] In a specific embodiment, in step 2, the annealing temperature is 1300-1500°C, and the holding time is 8-12h. For example, the annealing temperature is 1300°C, 1400°C, 1500°C, and the holding time is 8h, 9h, 10h, 11h, 12h.
[0038] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0039] The raw material powders used in the following examples are all commercially available products with a purity greater than 99.9%.
[0040] Embodiment 1:
[0041] Step 1: prepare YAG:Ce powder and YAG powder respectively; wherein the Ce ion concentration in the YAG:Ce powder is 0.01 at.%;
[0042] Step 2: dry pressing is used to press the YAG:Ce / YAG composite ceramic green body, first pressing the YAG powder, and then pressing the YAG:Ce powder, the mass ratio of the two is 1:1;
[0043] The green blank was vacuum sintered and annealed in sequence, with the sintering temperature at 1740°C and the holding time at 10h; the annealing temperature at 1300°C and the holding time at 10h;
[0044] Step 3: Use laser engraving technology to engrave a micro-convex lens array structure on the YAG:Ce surface of the composite ceramic. The bottom plane circle diameter of the micro-convex lens is 0.2mm and the height is 0.1mm. The final thickness of the composite fluorescent ceramic is 0.8mm.
[0045] The composite fluorescent ceramic is excited by 455nm blue light LD chip laser. When the blue light output power is 5W, its power density reaches 70.71W / mm 2 (The distance from the laser to the ceramic is 0.1mm), the fluorescent ceramic device emits light stably, and the luminous efficiency is 236.7lm / W (such as Figure 3 ); the luminous flux is as high as 1183.5lm, the beam divergence angle of the spatial light intensity distribution is 99.5°, which realizes beam convergence, and the overall transmittance of the prepared YAG:Ce / YAG composite ceramic is 80.02%.
[0046] Embodiment 2:
[0047] Step 1: preparing YAG:Ce powder and YAG powder respectively; wherein the Ce ion concentration in the YAG:Ce powder is 0.1 at.%;
[0048] Step 2: dry pressing is used to press the YAG:Ce / YAG composite ceramic green body, first pressing the YAG powder, and then pressing the YAG:Ce powder, the mass ratio of the two is 1:1;
[0049] The green blank is vacuum sintered and annealed in sequence. The sintering temperature is 1760℃, and the holding time is 13h; the annealing temperature is 1400℃, and the holding time is 10h;
[0050] Step 3: Use laser engraving technology to engrave a micro-convex lens array structure on the YAG:Ce surface of the composite ceramic. The bottom plane circle diameter of the micro-convex lens is 0.25mm and the height is 0.125mm. The final thickness of the composite fluorescent ceramic is 1mm.
[0051] The composite fluorescent ceramic is excited by 455nm blue light LD chip laser. When the blue light output power is 5W, its power density reaches 70.71W / mm 2 (The distance from the laser to the ceramic is 0.1mm), the fluorescent ceramic device emits light stably, and the luminous efficiency is 244.3lm / W (such as Figure 3 ); the luminous flux is as high as 1221.5lm, and the beam divergence angle of its spatial light intensity distribution is 92.5°, which realizes beam convergence (such as Figure 4 ), and the transmittance of the prepared YAG:Ce / YAG composite ceramic is 79.29% (as Figure 5 ).
[0052] Embodiment 3:
[0053] Step 1: prepare YAG:Ce powder and YAG powder respectively; wherein the Ce ion concentration in the YAG:Ce powder is 0.2at.%;
[0054] Step 2: dry pressing is used to press the YAG:Ce / YAG composite ceramic green body, first pressing the YAG powder, and then pressing the YAG:Ce powder, the mass ratio of the two is 1:1;
[0055] The green blank was vacuum sintered and annealed in sequence, with the sintering temperature at 1770°C and the holding time at 15h; the annealing temperature at 1500°C and the holding time at 12h;
[0056] Step 3: Use laser engraving technology to engrave a micro-convex lens array structure on the YAG:Ce surface of the composite ceramic. The bottom plane circle diameter of the micro-convex lens is 0.3mm and the height is 0.15mm. The final thickness of the composite fluorescent ceramic is 1.2mm.
[0057] The composite fluorescent ceramic is excited by 455nm blue light LD chip laser. When the blue light output power is 5W, its power density reaches 70.71W / mm 2 (The distance from the laser to the ceramic is 0.1mm), the fluorescent ceramic device emits light stably, and the luminous efficiency is 229.4lm / W. Figure 3 The luminous flux is as high as 1147 lm, and the beam divergence angle of the spatial light intensity distribution is 105.4°, which realizes beam convergence. The overall transmittance of the prepared YAG:Ce / YAG composite ceramic is 78.25%.
[0058] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A composite fluorescent ceramic for laser lighting, characterized in that: The composite fluorescent ceramic is obtained by co-firing a YAG:Ce fluorescent ceramic having a micro-convex lens array structure on the surface and a YAG transparent ceramic. The YAG:Ce fluorescent ceramic is used to improve the emission angle of photons and obtain collimated forward light. The YAG transparent ceramic is used to collect heat generated by the fluorescent layer and transfer the heat.
2. The composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: The doping concentration of Ce in the YAG:Ce fluorescent ceramic is 0.01-0.2 at %.
3. A method for preparing the composite fluorescent ceramic for laser lighting according to claim 1 or 2, characterized in that: The specific steps include: Step 1: Prepare YAG:Ce powder and YAG powder respectively; Step 2: dry pressing is used to press the YAG:Ce / YAG composite ceramic green body, and then vacuum sintering and annealing are performed in sequence to obtain the YAG:Ce / YAG composite ceramic; Step three: Use laser engraving technology to engrave a micro-convex lens array structure on the YAG:Ce surface of the composite ceramic. The bottom plane circle diameter of the micro-convex lens is 0.2-0.3mm and the height is 0.1-0.15mm, and finally a composite fluorescent ceramic with a thickness of 0.8-1.4mm is obtained.
4. The method for preparing the composite fluorescent ceramic for laser lighting according to claim 3, characterized in that: In step 2, YAG powder is pressed first, and then YAG:Ce powder is pressed; the mass ratio of the two is 1:
1.
5. The method for preparing the composite fluorescent ceramic for laser lighting according to claim 3, characterized in that: In step 2, the vacuum sintering temperature is 1740° C. to 1770° C., and the holding time is 10 to 15 hours.
6. The method for preparing the composite fluorescent ceramic for laser lighting according to claim 3, characterized in that: In step 2, the annealing temperature is 1300-1500° C., and the holding time is 8-12 hours.
Citation Information
Patent Citations
Ceramic fluorescent body capable of effectively eliminating edge aberration effect in white light LED light source packaging and preparation method thereof
CN104112812A
Composite fluorescent ceramic for reflection type laser illumination and preparation method of composite fluorescent ceramic
CN118108495A
Fluorescence transparent ceramic lens packaged white light LED
CN202423281U
Transmission screen, its manufacturing method, and back projection type projector
JP2004191429A
Phosphor lens and light emission device
JP2018146656A