Ceramic skeleton and preparation method and application thereof, and resin ceramic composite material and preparation method and application thereof
By regulating the porous structure and resin filling of the ceramic skeleton, high-strength, hardness and toughness resin ceramic composite materials are prepared, which solves the diversity of mechanical properties requirements and material wear problems of existing biomedical materials, and improves the service life of dentures.
Patent Information
- Application Number
- CN202411169968.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
During the production process of existing biomedical materials, due to different mechanical properties such as strength, hardness, toughness, etc., the production methods are diverse, which increases costs and time. In addition, all-ceramic dentures and resin dentures on the market have their own shortcomings, which are not suitable for rapid wear and unsuitable. Match with human teeth.
A ceramic skeleton with a porous structure and a preparation method thereof is provided. By regulating the porous structure and resin filling of the ceramic skeleton, resin ceramic composite materials with high strength, hardness and toughness are prepared, which are suitable for biomedical materials such as dentures.
The mechanical properties of the ceramic skeleton are adjusted, adapt to different uses needs, improve the service life of dentures, and through the preparation of resin-ceramic composite materials, the advantages of ceramics and resins are combined to meet the mechanical properties requirements of biomedical materials.
Smart Images

Figure CN119059838A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to a ceramic skeleton and a preparation method and application thereof, and a resin-ceramic composite material and a preparation method and application thereof. Background Art
[0002] Biomedical materials are materials used to diagnose, treat, repair or replace damaged tissues and organs or enhance their functions. Biomedical materials can be divided into bone, tooth, joint, tendon and other skeletal-muscle system repair materials, skin, breast, esophagus, respiratory tract, bladder and other soft tissue materials, artificial heart valves, blood vessels, cardiovascular catheters and other cardiovascular system materials, blood purification membranes and separation membranes, gas selective permeable membranes, corneal contact lenses and other medical membrane materials, tissue adhesives and suture materials, drug release carrier materials, clinical diagnosis and biosensor materials, dental materials, etc.
[0003] Biomedical materials for different purposes have different requirements for mechanical properties such as strength, hardness, and toughness. This requires that during the production and manufacturing process of biomedical materials, multiple production or processing methods must be adopted to obtain a variety of biomaterials to meet the requirements of different mechanical properties, thereby increasing the labor and time costs of production. Summary of the invention
[0004] The purpose of the present invention is to provide a ceramic skeleton and a preparation method and application thereof, a resin ceramic composite material and a preparation method and application thereof. The ceramic skeleton provided by the present invention has various types of porous structures, and the mechanical properties are adjustable and controllable.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a ceramic skeleton having a porous structure;
[0007] The porous structure includes one or more of a connected pore structure and a through-pore structure;
[0008] The interconnected hole structure is formed by a plurality of holes being interconnected;
[0009] The through hole structure includes one or more of a unidirectional through hole structure and a divergent through hole structure.
[0010] Preferably, the holes in the interconnecting hole structure are regular and / or irregular holes.
[0011] Preferably, the aperture of the holes in the interconnecting hole structure increases successively from one end to the other, or the aperture of the holes increases first and then decreases from one end to the other, or the aperture of the holes decreases first and then increases from one end to the other.
[0012] Preferably, the pore sizes of the holes in the interconnected pore structure are independently in the range of less than 1000 μm.
[0013] Preferably, the one-way through hole structure is composed of a plurality of through holes extending from one end to the other end.
[0014] Preferably, the divergent through-hole structure comprises a plurality of through-holes which radiate from a starting position inside the ceramic skeleton to the surrounding areas.
[0015] Preferably, the divergent through-hole structure comprises a three-dimensional through-hole structure;
[0016] The three-dimensional through hole structure is composed of a plurality of three-dimensional through holes penetrating upward, downward, leftward, rightward, and rearward.
[0017] Preferably, the aperture of each through hole in the one-way through hole structure increases independently from one end to the other end, or the aperture of each through hole increases independently from one end to the other end and then decreases, or the aperture of each through hole decreases independently from one end to the other end and then increases.
[0018] Preferably, the pore size range of each through hole in the one-way through hole structure is independently less than 1000 μm.
[0019] Preferably, the aperture of each through hole in the divergent through hole structure increases gradually from a starting position to the surroundings to form a trumpet shape, or the aperture of each through hole decreases gradually from a starting position to the surroundings, or the aperture of each through hole increases first and then decreases from a starting position to the surroundings, or the aperture of each through hole decreases first and then increases from a starting position to the surroundings.
[0020] Preferably, the pore size range of each through hole in the divergent through hole structure is independently less than 1000 μm.
[0021] Preferably, the aperture of each three-dimensional through hole in the three-dimensional through hole structure independently increases gradually from the middle to the surroundings to form a trumpet shape, or the aperture of each three-dimensional through hole independently decreases gradually from the middle to the surroundings, or the aperture of each three-dimensional through hole independently increases first and then decreases from the middle to the surroundings, or the aperture of each three-dimensional through hole independently decreases first and then increases from the middle to the surroundings.
[0022] Preferably, the pore size range of each three-dimensional through-hole in the three-dimensional through-hole structure is independently less than 1000 μm.
[0023] The present invention provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0024] Mixing a main raw material, a binder and a solvent to obtain a slurry; the main raw material includes one or more of a bio-inert ceramic material and a bio-active ceramic material;
[0025] Casting the slurry to obtain a cast sheet;
[0026] laminating the cast sheet to obtain a laminated sheet;
[0027] The laminated sheets are sintered to obtain a ceramic skeleton.
[0028] The present invention provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0029] Mixing a main raw material and a solvent to obtain a ceramic slurry; the main raw material includes one or more of a bio-inert ceramic material and a bio-active ceramic material;
[0030] Freezing the ceramic slurry to obtain a frozen block;
[0031] Drying the frozen block to obtain a dried sample block;
[0032] The dried sample is sintered to obtain a ceramic skeleton.
[0033] The present invention provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0034] Mixing main raw materials to obtain ceramic powder; the main raw materials include one or more of biologically inert ceramic materials and biologically active ceramic materials;
[0035] Dry pressing and / or isostatic pressing the ceramic powder to obtain a green body;
[0036] The green body is sintered to obtain a ceramic skeleton.
[0037] The present invention provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0038] Mixing main raw materials to obtain a mixture; the main raw materials include one or more of a bio-inert ceramic material and a bio-active ceramic material;
[0039] kneading the mixed material, the binder and the solvent to obtain a kneaded material;
[0040] The kneaded material is aged and then kneaded to obtain a kneaded mud block;
[0041] The conditioned clay block is segmented to obtain clay segments;
[0042] Extruding the mud segment to obtain a wet blank;
[0043] Drying the wet blank to obtain a dry blank;
[0044] The dry blank is sintered to obtain a ceramic skeleton.
[0045] The present invention provides the use of the ceramic skeleton described in the above technical solution or the ceramic skeleton prepared by the preparation method described in the above technical solution in the preparation of biomedical materials.
[0046] Preferably, the biomedical material comprises a denture, an artificial eye or a bionic bone.
[0047] The present invention provides a resin-ceramic composite material, comprising a ceramic skeleton and a resin filled in the porous structure of the ceramic skeleton; the ceramic skeleton is the ceramic skeleton described in the above technical solution or a ceramic skeleton prepared by the preparation method described in the above technical solution.
[0048] Preferably, the raw materials for preparing the resin include one or more of monofunctional acrylates and multifunctional acrylates.
[0049] The present invention provides a method for preparing the resin-ceramic composite material described in the above technical solution, comprising the following steps:
[0050] The ceramic skeleton is immersed in a resin precursor solution and solidified to obtain a resin-ceramic composite material.
[0051] Preferably, the curing pressure is 0.1-500 MPa; the curing temperature is 10-180° C.; and the curing heat preservation and pressure holding time is 1 min-48 h.
[0052] The present invention provides the use of the resin-ceramic composite material described in the above technical solution or the resin-ceramic composite material prepared by the preparation method described in the above technical solution in the preparation of biomedical materials.
[0053] Preferably, the biomedical material comprises a denture, an artificial eye or a bionic bone.
[0054] The present invention provides a ceramic skeleton having a porous structure. In the present invention, ceramic skeletons with different porous structures have different hardness and strength, and can meet the needs of biomedical materials with different uses.
[0055] The present invention provides a method for preparing the ceramic skeleton described in the above technical scheme. In the present invention, the main raw materials of the ceramic skeleton include one or more of bioinert ceramic materials and bioactive ceramic materials. As a preferred scheme, zirconium oxide, feldspar, sodium aluminum silicate, hydroxyapatite, etc. can be used as denture materials, and hydroxyapatite, calcium phosphate and zirconium oxide with better biocompatibility can be used as a variety of bionic bone materials, which can meet the needs of biomedical materials for different purposes.
[0056] The present invention provides a resin ceramic composite material, comprising a ceramic skeleton and a resin filled in the porous structure of the ceramic skeleton. The present invention can adjust the hardness, strength and toughness of the resin ceramic composite material by combining ceramic skeletons with different porous structures and different resins, and can be applied to biomedical materials such as artificial teeth, artificial eyes or bionic bones.
[0057] A further preferred solution is that the resin ceramic composite material provided by the present invention has high hardness and strength on the outside and excellent toughness on the inside, which can increase the service life of the denture. The mainstream all-ceramic dentures on the market are generally made of zirconia ceramics, which have high strength, high elastic modulus, high hardness and wear resistance of ceramics. The hardness of zirconia ceramics is second only to diamonds. It will seriously wear normal human teeth during use and is not suitable for matching with normal teeth. The wear resistance of resin dentures is less than that of normal teeth. They will quickly wear out during use, resulting in a lower lifespan, and are not suitable for matching with human teeth. The present invention combines the characteristics of the two materials to prepare a resin ceramic composite material. The composite material has high strength to meet the use strength requirements, and the hardness and wear resistance are also close to those of human teeth, thereby increasing the service life of the denture. Moreover, the resin ceramic composite material provided by the present invention can be directly turned according to customer needs and used as a denture, which is suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 A schematic diagram of a ceramic skeleton structure with through holes whose pore diameter increases from one end to the other end;
[0059] Figure 2 A schematic diagram of a ceramic skeleton structure with through holes, the aperture of which first decreases and then increases from one end to the other end;
[0060] Figure 3 A schematic diagram of a ceramic skeleton structure with through holes, the aperture of which increases first and then decreases from one end to the other end;
[0061] Figure 4 A schematic diagram of a ceramic skeleton structure having through holes from one end to the other end;
[0062] Figure 5 Schematic diagram of a ceramic skeleton structure with through holes with various changing trends (small holes on both end faces);
[0063] Figure 6 Schematic diagram of a ceramic skeleton structure with through holes;
[0064] Figure 7 Schematic diagram of a ceramic skeleton structure with three-dimensional interconnected pores;
[0065] Figure 8 Schematic diagram of a ceramic skeleton structure with three-dimensional through holes;
[0066] Fig. 9 Schematic diagram of a ceramic skeleton structure with through holes with various changing trends (large holes on both end faces);
[0067] Fig.10 Schematic diagram of a ceramic skeleton structure with interconnecting pores that first decrease and then increase;
[0068] Fig.11 Schematic diagram of a ceramic skeleton structure with unidirectionally enlarged interconnected pores;
[0069] Fig.12 A schematic diagram of a ceramic skeleton structure having interconnected pores with various changing trends;
[0070] Fig.13 A schematic diagram of a ceramic skeleton structure with three-dimensional through holes, wherein the pore size gradually increases from the middle to the surrounding areas;
[0071] Fig.14 A schematic diagram of a ceramic skeleton structure with divergent through holes, wherein the pore size gradually increases from the inside to the surroundings;
[0072] Fig.15 Schematic diagram of a ceramic skeleton structure with interconnected pores whose pore size increases first and then decreases;
[0073] Fig.16 This is the SEM image of the ceramic skeleton prepared in Example 1. DETAILED DESCRIPTION
[0074] The present invention provides a ceramic skeleton having a porous structure;
[0075] The porous structure includes one or more of a connected pore structure and a through-pore structure;
[0076] The interconnected hole structure is formed by a plurality of holes being interconnected;
[0077] The through hole structure includes one or more of a unidirectional through hole structure and a divergent through hole structure.
[0078] The ceramic skeleton provided by the present invention has a porous structure; the porous structure includes one or more of a connected pore structure and a through-pore structure. In the present invention, the connected pore structure is composed of pores that are interconnected, and the pores are open or closed. In the present invention, the through-pore structure is composed of holes that penetrate from one end to the other end.
[0079] In the present invention, the holes in the interconnected pore structure are regular and / or irregular holes. In the present invention, the pore size of the holes in the interconnected pore structure increases from one end to the other end, or the pore size of the holes increases first and then decreases from one end to the other end, or the pore size of the holes decreases first and then increases from one end to the other end. In the present invention, the pore size range of the holes in the interconnected pore structure is independently preferably less than 1000 μm, more preferably 0.1 to 1 μm, 1 to 50 μm or 100 to 1000 μm.
[0080] In the present invention, the through hole structure includes one or more of a unidirectional through hole structure and a divergent through hole structure.
[0081] In the present invention, the one-way through hole structure is composed of a plurality of through holes from one end to the other end. In a specific embodiment of the present invention, the aperture of each through hole in the one-way through hole structure increases independently from one end to the other end, or the aperture of each through hole increases independently from one end to the other end and then decreases, or the aperture of each through hole decreases independently from one end to the other end and then increases. In the present invention, the aperture range of each through hole in the one-way through hole structure is preferably less than 1000 μm, more preferably 0.1 to 1 μm, 1 to 50 μm or 100 to 1000 μm.
[0082] In the present invention, the divergent through-hole structure includes a plurality of through-holes that diverge from a starting position inside a ceramic skeleton to the surroundings. In a specific embodiment of the present invention, the aperture of each through-hole in the divergent through-hole structure independently increases gradually from the starting position to the surroundings to form a trumpet shape, or the aperture of each through-hole independently decreases gradually from the starting position to the surroundings, or the aperture of each through-hole independently increases first and then decreases from the starting position to the surroundings, or the aperture of each through-hole independently decreases first and then increases from the starting position to the surroundings. In the present invention, the aperture range of each through-hole in the divergent through-hole structure is independently preferably less than 1000 μm, more preferably 0.1-1 μm, 1-50 μm or 100-1000 μm.
[0083] In the present invention, the divergent through-hole structure preferably includes a three-dimensional through-hole structure; the three-dimensional through-hole structure is composed of a number of three-dimensional through-holes that penetrate up, down, left, right, front, and back. In a specific embodiment of the present invention, the aperture of each three-dimensional through-hole in the three-dimensional through-hole structure independently increases gradually from the middle to the surroundings to form a trumpet shape, or the aperture of each three-dimensional through-hole independently decreases gradually from the middle to the surroundings, or the aperture of each three-dimensional through-hole independently increases first and then decreases from the middle to the surroundings, or the aperture of each three-dimensional through-hole independently decreases first and then increases from the middle to the surroundings. In the present invention, the aperture range of each three-dimensional through-hole in the three-dimensional through-hole structure is independently preferably less than 1000μm, more preferably 0.1-1μm, 1-50μm or 100-1000μm.
[0084] In a specific embodiment of the present invention, the structure of the ceramic skeleton includes: Figure 1 As shown in FIG. 1 , the pore size increases from one end to the other end, and the ceramic skeleton with through holes is as follows: Figure 2 As shown in the figure, the pore size decreases from one end to the other and then increases. The ceramic skeleton with through holes, such as Figure 3 As shown in the figure, the pore size increases from one end to the other and then decreases. The ceramic skeleton with through holes, such as Figure 4 The ceramic skeleton having through holes from one end to the other end as shown in Figure 5 The ceramic skeleton with various through holes (small holes on both ends) as shown in FIG. Figure 6 The ceramic skeleton with through holes as shown in Figure 7 The ceramic skeleton with three-dimensional interconnected pores shown in FIG. Figure 8 The ceramic skeleton with three-dimensional through-holes shown in FIG. Fig. 9 The ceramic skeleton with various through holes (large holes on both ends) as shown in FIG. Fig.10 The ceramic skeleton with the interconnecting holes first reduced and then increased as shown in Fig.11 The ceramic skeleton with unidirectionally enlarged interconnected pores shown in FIG. Fig.12 The ceramic skeleton with interconnected pores having various changing trends, such as Fig.13 The pore size gradually increases from the middle to the surrounding area, and the ceramic skeleton with three-dimensional through holes, such as Fig.14 The pore size gradually increases from the inside to the surrounding area. The ceramic skeleton with divergent through-holes and Fig.15 One or more of the ceramic skeletons with interconnected pores whose pore diameter increases first and then decreases.
[0085] The present invention provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0086] Mixing a main raw material, a binder and a solvent to obtain a slurry; the main raw material includes one or more of a bio-inert ceramic material and a bio-active ceramic material;
[0087] Casting the slurry to obtain a cast sheet;
[0088] laminating the cast sheet to obtain a laminated sheet;
[0089] The laminated sheets are sintered to obtain a ceramic skeleton.
[0090] The present invention mixes a main raw material, a binder and a solvent to obtain a slurry. In the present invention, the main raw material includes one or more of a bio-inert ceramic material and a bio-active ceramic material. In the present invention, the slurry preferably also includes one or more of a dispersant, a plasticizer and a pore-forming agent.
[0091] In the present invention, the bio-inert ceramic material preferably includes one or more of zirconium oxide, aluminum oxide, quartz, lithium disilicate, glass powder, magnesium aluminum spinel, sodium aluminum silicate, feldspar, silicon carbide, carbon nanostructure and nitride; the carbon nanostructure preferably includes carbon nanotubes; the nitride preferably includes one or more of titanium nitride, zirconium nitride and chromium nitride. In the present invention, the bioactive ceramic material preferably includes one or more of hydroxyapatite, fluoroapatite, bioglass ceramics (Na-Ca-Si glass), AW glass ceramics, calcium phosphate, calcium carbonate and calcium sulfate; the bioglass ceramics preferably include Na-Ca-Si glass. In the present invention, the feldspar preferably includes one or more of sodium feldspar, potassium feldspar and potassium sodium feldspar. In the present invention, the D50 particle size of the main raw material is preferably 0.05 to 1500 μm. In the present invention, the particle size of the raw material refers to the value of D50. In the present invention, the binder preferably includes one or more of polyvinyl alcohol (PVA) aqueous solution and hydroxypropyl methylcellulose; the concentration of the PVA aqueous solution is preferably 1-10%, more preferably 3-5%; the average molecular weight of polyvinyl alcohol is preferably 155000-182000; the viscosity range of the hydroxypropyl methylcellulose is preferably 3500-5600. In the present invention, the dispersant preferably includes one or more of triammonium citrate, sodium polyacrylate and glycerol; the molecular weight of the sodium polyacrylate is preferably 4000-10000. In the present invention, the plasticizer preferably includes polyethylene glycol (PEG); the molecular weight of the polyethylene glycol is preferably 380-420, more preferably 400. In the present invention, the pore-forming agent preferably includes one or more of polymethyl methacrylate (PMMA), corn starch and potato flour. In the present invention, the molecular weight of the PMMA is preferably 90000-120000, more preferably 100000-120000. In the present invention, the particle size of the pore former is preferably 0.5 to 1200 μm. In the present invention, the solvent is preferably water or anhydrous ethanol.
[0092] In the present invention, the mass ratio of the main raw material, the binder and the solvent is preferably (60-120): (6-20): (70-120), and more preferably (60-105): (6-20): (72-120). In the present invention, when the slurry includes a dispersant, a plasticizer and a pore-forming agent, the mass ratio of the main raw material, the binder, the dispersant, the plasticizer, the pore-forming agent and water is preferably (60-120): (6-20): (0.1-12): (0.1-15): (2-50): (70-120), and more preferably (60-105): (6-20): (0.1-10): (0.1-15): (2-45): (72-120).
[0093] In the present invention, the mixing is preferably wet ball milling. In the present invention, the rotation speed of the wet ball milling is preferably 10 to 1000 r / min, more preferably 10 to 900 r / min; the time of the wet ball milling is preferably 0.5 to 30 hours, more preferably 1 to 24 hours; the grinding balls used in the wet ball milling are preferably alumina balls or zirconia balls, more preferably zirconia balls; the ball-to-material mass ratio is preferably 1: (0.5 to 1.2), more preferably 1: (0.8 to 1.2). In a specific embodiment of the present invention, the grinding balls used in the wet ball milling are zirconia balls; the ball-to-material mass ratio is 1: 0.8.
[0094] In a specific embodiment of the present invention, different casting slurries are obtained by adjusting the type, addition amount and pore size of the pore-forming agent.
[0095] After obtaining the slurry, the present invention performs tape casting on the casting slurry to obtain a cast sheet. In the present invention, the tape casting is preferably performed in a tape casting machine. In a specific embodiment of the present invention, by adjusting the height of the scraper, cast sheets of different thicknesses can be obtained.
[0096] After obtaining the cast sheet, the present invention laminates the cast sheet to obtain a laminated sheet. In the present invention, the lamination is preferably carried out in a warm isostatic press; the lamination pressure is preferably 8 to 260 MPa, more preferably 20 to 200 MPa, and further preferably 90 to 150 MPa; the lamination temperature is preferably 30 to 60°C, more preferably 35 to 55°C, and further preferably 40 to 50°C; the heat preservation and pressure holding time is preferably 0.5 to 25 min, and more preferably 1 to 15 min. In the present invention, the lamination is adjusted according to the pore structure of the ceramic skeleton. In a specific embodiment of the present invention, the cast sheets formed by the same type of casting slurry are first laminated to obtain a cast sheet layer, and then the cast sheet layers formed by different types of casting slurries are laminated according to the pore structure of the ceramic skeleton; the thickness of each cast sheet layer is the same or different.
[0097] After obtaining the laminated sheet, the present invention sintered the laminated sheet to obtain a ceramic skeleton. In the present invention, the laminated sheet is preferably cut into a cuboid before sintering. In the present invention, the sintering is preferably carried out in a high-temperature furnace. In the present invention, the sintering procedure preferably includes: heating from room temperature to 290°C after 240 minutes, keeping warm at 290°C for 60 minutes, heating to 410°C after 120 minutes, keeping warm at 410°C for 1 hour, heating to 700-1650°C after 180-300 minutes, and keeping warm at 700-1650°C for 1-5 hours. The present invention has no special requirements for the sintering atmosphere, and any sintering atmosphere known in the art can be used. In a specific embodiment of the present invention, the sintering atmosphere is air. The present invention performs sufficient debinding before the temperature reaches 500°C, and performs final sintering at 700-1650°C. In the sintering process of the present invention, the pore-forming agent is decomposed to form pores, and a ceramic skeleton with different porous structures can be obtained by adjusting the type, addition amount and pore diameter of the pore-forming agent.
[0098] The present invention also provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0099] Mixing a main raw material and a solvent to obtain a ceramic slurry; the main raw material includes one or more of a bio-inert ceramic material and a bio-active ceramic material;
[0100] Freezing the ceramic slurry to obtain a frozen block;
[0101] Drying the frozen block to obtain a dried sample block;
[0102] The dried sample is sintered to obtain a ceramic skeleton.
[0103] The present invention mixes the main raw material and the solvent to obtain a ceramic slurry. In the present invention, the ceramic slurry preferably also includes one or more of a binder, a dispersant, a plasticizer and a pore former. In the present invention, the composition of the main raw material, the solvent, the binder, the dispersant, the plasticizer and the pore former is consistent with that described above, and will not be repeated here; the preparation method of the ceramic slurry is consistent with the preparation method of the slurry described above, and will not be repeated here. In a specific embodiment of the present invention, different ceramic slurries are obtained by adjusting the addition amount and pore size of the pore former.
[0104] After obtaining the ceramic slurry, the present invention freezes the ceramic slurry to obtain a frozen block. In the present invention, the freezing temperature is preferably -20 to -150°C, more preferably -20 to -120°C. In the present invention, the freezing method of different ceramic slurries during the freezing process is adjusted according to the pore structure of the ceramic skeleton.
[0105] After obtaining the frozen block, the present invention dries the frozen block to obtain a dried sample block. In the present invention, the drying is preferably vacuum freeze drying; the drying temperature is preferably -20 to 50°C, more preferably -20 to 35°C; the drying pressure is preferably 20 to 5000Pa, more preferably 20 to 1000Pa; the drying time is preferably 0.5 to 48h, more preferably 1 to 36h. In the vacuum freeze drying process of the present invention, water volatilization will form pores, and freeze-dried samples with different pore structures can be obtained by adjusting the amount of water in the slurry, the number of pouring times and the shape of the mold.
[0106] After obtaining the dried sample, the present invention sintered the dried sample to obtain a ceramic skeleton. In the present invention, the sintering procedure preferably includes: heating from room temperature to 290°C after 240 minutes, keeping warm at 290°C for 60 minutes, heating to 410°C after 120 minutes, keeping warm at 410°C for 1 hour, heating to 700-1650°C after 180-300 minutes, and keeping warm at 700-1650°C for 1-5 hours. The present invention has no special requirements for the sintering atmosphere, and any sintering atmosphere known in the art can be used. In a specific embodiment of the present invention, the sintering atmosphere is air. The present invention performs sufficient debinding before the temperature reaches 500°C, and performs final sintering at 700-1650°C. During the sintering process of the present invention, the pore-forming agent decomposes to form pores. By adjusting the type, addition amount and pore size of the pore-forming agent and the amount of water in the slurry, a ceramic skeleton with different porous structures can be obtained.
[0107] The present invention also provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0108] Mixing main raw materials to obtain ceramic powder; the main raw materials include one or more of biologically inert ceramic materials and biologically active ceramic materials;
[0109] Dry pressing and / or isostatic pressing the ceramic powder to obtain a green body;
[0110] The green body is sintered to obtain a ceramic skeleton.
[0111] The present invention mixes the main raw materials to obtain ceramic powder. In the present invention, the raw materials for preparing the ceramic powder preferably also include one or more of a binder, a pore former and a solvent. In the present invention, the composition of the main raw material, the binder, the pore former and the solvent is consistent with that described above, and will not be repeated here.
[0112] In the present invention, the binder is preferably a 3wt% PVA aqueous solution; the mass of the binder is preferably 5-30% of the mass of the main raw material, more preferably 5-29%; the solvent is preferably water or anhydrous ethanol; the mass ratio of the solvent to the main raw material is preferably 1-3:1. In the present invention, when the raw materials for preparing the ceramic powder include a solvent, the mixing preferably includes wet ball milling and drying in sequence. In the present invention, the rotation speed of the wet ball mill is preferably 10-1000r / min, more preferably 10-900r / min; the time of the wet ball milling is preferably 0.5-30h, more preferably 1-24h; the grinding balls used in the wet ball milling are preferably alumina balls or zirconia balls, more preferably zirconia balls; the ball-to-material mass ratio is preferably 1:(0.5-1.2), more preferably 1:(0.8-1.2). In a specific embodiment of the present invention, the grinding balls used in the wet ball milling are zirconia balls; the ball-to-material mass ratio is 1:0.8. In the present invention, the drying temperature is preferably 45-110°C, more preferably 47-105°C.
[0113] After obtaining the ceramic powder, the present invention performs dry pressing and / or isostatic pressing on the ceramic powder to obtain a green body. In the present invention, the dry pressing pressure is preferably 2 to 30 MPa, more preferably 2 to 28 MPa; the dry pressing time is preferably 10 to 180 s, more preferably 20 to 150 s. In the present invention, the isostatic pressing pressure is preferably 50 to 300 MPa; the isostatic pressing is preferably cold isostatic pressing or hot isostatic pressing; the isostatic pressing temperature is preferably room temperature; the isostatic pressing time is preferably 30 to 1800 s, more preferably 30 to 1200 s. In the present invention, when the ceramic powder is dry pressed and isostatically pressed, it is preferred to perform dry pressing and isostatic pressing sequentially.
[0114] After obtaining the green body, the present invention sintered the green body to obtain a ceramic skeleton. In the present invention, the sintering process is consistent with that described above and will not be repeated here.
[0115] The present invention also provides a method for preparing the ceramic skeleton described in the above technical solution, comprising the following steps:
[0116] Mixing main raw materials to obtain a mixture; the main raw materials include one or more of a bio-inert ceramic material and a bio-active ceramic material;
[0117] kneading the mixed material, the binder and the solvent to obtain a kneaded material;
[0118] The kneaded material is aged and then kneaded to obtain a kneaded mud block;
[0119] The conditioned clay block is segmented to obtain clay segments;
[0120] Extruding the mud segment to obtain a wet blank;
[0121] Drying the wet blank to obtain a dry blank;
[0122] The dry blank is sintered to obtain a ceramic skeleton.
[0123] The present invention mixes the main raw materials to obtain a mixture. In the present invention, the composition of the main raw materials is consistent with that described above, and will not be repeated here. In the present invention, the mixing is preferably carried out in a mixer. In the mixing process of the present invention, a pore former and a solid binder are preferably added. In the present invention, the composition of the pore former is consistent with that described above, and will not be repeated here. In the present invention, the mass ratio of the pore former to the main raw material is preferably 1 to 50:100 to 120, and more preferably 1:10. In the present invention, the solid binder preferably includes hydroxypropyl methylcellulose; the mass of the solid binder is preferably 1 to 6% of the mass of the main raw material, and more preferably 3.3 to 5%.
[0124] After obtaining the mixed material, the present invention kneads the mixed material, the liquid binder and the solvent to obtain a kneaded material. In the present invention, a dispersant is preferably added during the kneading process. In the present invention, the composition of the solvent and the dispersant is consistent with that described above, and will not be repeated here. In the present invention, the liquid binder is preferably a PVA aqueous solution; the concentration of the PVA aqueous solution is preferably 3wt%; the mass of the PVA aqueous solution is preferably 1-6% of the mass of the main raw material, and more preferably 1-5.5%. The present invention uses a liquid binder and a solid binder, and the effect is better. In the present invention, the dispersant is preferably glycerol; the mass of the glycerol is preferably 0.3-3% of the mass of the main raw material, and more preferably 0.3-2.9%. In the present invention, the mass ratio of the solvent to the main raw material is preferably 20-30:100-120, and more preferably 26.5:100. In the present invention, the kneading is preferably carried out in a kneader. In the present invention, the kneading speed is preferably 12-30 revolutions per minute.
[0125] After obtaining the kneaded material, the present invention ages the kneaded material and then kneads it to obtain a kneaded mud block. In the present invention, the aging temperature is preferably 10 to 30°C, more preferably 10 to 28°C; the aging time is preferably 12 to 48 hours, more preferably 12 to 36 hours. In the present invention, the kneading is preferably carried out in a mud kneading machine. In the present invention, the extrusion speed of the mud kneading machine is preferably 30 to 80 cm / min.
[0126] After obtaining the kneaded mud block, the present invention performs mud segmentation on the kneaded mud block to obtain mud segments. In the present invention, the mud segmentation is preferably performed in a mud segmentation machine. In the present invention, the extrusion speed of the mud segmentation machine is preferably 20 to 60 cm / min.
[0127] After obtaining the clay segments, the present invention performs extrusion molding on the clay segments to obtain wet blanks. In the present invention, the extrusion molding is preferably performed in an extrusion molding machine. In the present invention, the extrusion speed of the extrusion molding machine is preferably 30 to 100 cm / min.
[0128] After obtaining the wet blank, the present invention dries the wet blank to obtain a dry blank. In the present invention, the drying is preferably microwave drying. In the present invention, the microwave power of the microwave drying is preferably 1 to 5 kW, and the microwave drying time is preferably 50 to 120 seconds.
[0129] After obtaining the dry blank, the present invention sintered the dry blank to obtain a ceramic skeleton. In the present invention, the sintering process is consistent with that described above and will not be repeated here.
[0130] In a specific embodiment of the present invention, the method for preparing the ceramic skeleton also includes gel injection molding, organic template method, foaming method, particle accumulation method or additive manufacturing method.
[0131] The present invention provides the use of the ceramic skeleton described in the above technical solution or the ceramic skeleton prepared by the preparation method described in the above technical solution in the preparation of biomedical materials. In the present invention, the biomedical material preferably includes artificial teeth, artificial eyes or bionic bones.
[0132] The present invention provides a resin-ceramic composite material, comprising a ceramic skeleton and a resin filled in the porous structure of the ceramic skeleton; the ceramic skeleton is the ceramic skeleton described in the above technical solution or a ceramic skeleton prepared by the preparation method described in the above technical solution.
[0133] In the present invention, the raw materials for preparing the resin preferably include one or more of monofunctional acrylates and multifunctional acrylates. In the present invention, the multifunctional acrylate preferably includes one or more of difunctional acrylates and trifunctional acrylates. In the present invention, the monofunctional acrylate preferably includes hydroxyethyl methacrylate, hydroxypropyl methacrylate, and methyl methacrylate; the difunctional acrylate preferably includes bisphenol A-dimethacrylate glycidyl ester, diurethane dimethacrylate, triethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethoxy bisphenol A-dimethacrylate, tetraethoxy bisphenol A-dimethacrylate, and decaethoxy bisphenol A-dimethacrylate; the trifunctional acrylate preferably includes pentaerythritol triacrylate, trimethylolpropane trimethacrylate, and trimethylolpropane triacrylate.
[0134] In a specific embodiment of the present invention, the raw materials for preparing the resin preferably include one or more of bisphenol A-glycidyl dimethacrylate (Bis-GMA, molecular weight 512.59), diurethane dimethacrylate (UDMA, molecular weight 470.56) and triethylene glycol dimethacrylate (TEGDMA, molecular weight 286.321), and more preferably Bis-GMA, UDMA and TEGDMA. In the present invention, the mass ratio of Bis-GMA, UDMA and TEGDMA is preferably (2-3.5): (3-5): (2-3.5), and more preferably (2.5-3.5): (3-5): (2.5-3.5). In the present invention, the raw materials for preparing the resin preferably also include an initiator; the initiator preferably includes benzoyl peroxide (BPO); the mass fraction of the initiator in the raw materials for preparing the resin is preferably 0.1-1.0%, and more preferably 0.55-1.0%. In the present invention, the raw material for preparing the resin preferably also includes a PVA aqueous solution; the concentration of the PVA aqueous solution is preferably 3-15wt%, more preferably 5-15wt%; the molecular weight of PVA in the PVA aqueous solution is preferably 155000-182000, more preferably 155000-180000. In the present invention, the volume content of the PVA aqueous solution in the raw material for preparing the resin is preferably 60-95%, more preferably 65-91%.
[0135] The present invention provides a method for preparing the resin-ceramic composite material described in the above technical solution, comprising the following steps:
[0136] The ceramic skeleton is immersed in a resin precursor solution and solidified to obtain a resin-ceramic composite material.
[0137] In the present invention, the raw materials for preparing the resin precursor solution preferably include one or more of bisphenol A-glycidyl dimethacrylate (Bis-GMA), diurethane dimethacrylate (UDMA) and triethylene glycol dimethacrylate (TEGDMA), and more preferably Bis-GMA, UDMA and TEGDMA. In the present invention, the mass ratio of Bis-GMA, UDMA and TEGDMA is preferably (2-3.5): (3-5): (2-3.5), and more preferably (2.5-3.5): (3-5): (2.5-3.5). In the present invention, the raw materials for preparing the resin precursor solution preferably also include an initiator; the initiator preferably includes benzoyl peroxide (BPO); the mass fraction of the initiator in the raw materials for preparing the resin is preferably 0.1-1.0%, and more preferably 0.55-1.0%. In the present invention, the raw materials for preparing the resin precursor solution preferably also include a PVA aqueous solution; the concentration of the PVA aqueous solution is preferably 3-15wt%, more preferably 5-15wt%; the molecular weight of PVA in the PVA aqueous solution is preferably 155000-182000, more preferably 155000-180000. In the present invention, the volume content of the PVA aqueous solution in the resin precursor solution is preferably 60-95%, more preferably 65-91%.
[0138] In the present invention, the method for preparing the PVA aqueous solution preferably comprises: mixing PVA and water to obtain the PVA aqueous solution. In the present invention, the mixing temperature is preferably 85 to 95° C., more preferably 90° C.; the mixing time is preferably 3 to 12 hours, more preferably 4 to 10 hours.
[0139] In the present invention, the ceramic skeleton is preferably further modified before being impregnated; the modification liquid used for the modification is a silane modification liquid; the silane modification liquid includes anhydrous ethanol, distilled water, acetic acid and γ-methacryloxypropyltrimethoxysilane (KH570); the mass ratio of anhydrous ethanol, distilled water, acetic acid and KH570 is preferably (0.8-1.2): (0.7-1.2): (0.001-0.015): (0.002-0.01). In the present invention, the impregnation is preferably vacuum infiltration. In the present invention, the volume ratio of the ceramic skeleton and the resin precursor liquid is preferably (6-8): (2-4), more preferably (6.5-7.5): (2.5-3.5). In the present invention, the immersion temperature is preferably 10-37°C, more preferably 20-30°C; the immersion time is preferably 24-240h, more preferably 36-200h; the immersion pressure is preferably 1-10000Pa, more preferably 100-5000Pa.
[0140] In the present invention, the curing is preferably carried out in a warm isostatic press; the curing pressure is preferably 0.1 to 500 MPa, more preferably 50 to 300 MPa; the curing temperature is preferably 10 to 180°C, more preferably 60 to 120°C, further preferably 80 to 100°C; the curing heat and pressure holding time is preferably 1 min to 48 h, more preferably 6 to 36 h.
[0141] In the present invention, when the raw material for preparing the resin precursor solution includes a PVA aqueous solution, the curing preferably includes gelation, drying, normal pressure curing and water absorption treatment performed in sequence. In the present invention, the gelation preferably includes freezing and thawing performed in sequence; the freezing temperature is preferably -20°C to -150°C, more preferably -20°C to -120°C; the freezing time is preferably 0.5 to 48h, more preferably 1 to 12h; the thawing is preferably performed at room temperature. In the present invention, the number of freezing and thawing is preferably 2 to 3 times. The present invention cross-links PVA multiple times through gelation to obtain a PVA hydrogel with certain strength, high elasticity and lubricity. In the present invention, the drying is preferably vacuum freeze drying; the drying pressure is preferably 20 to 5000Pa, more preferably 20 to 1000Pa; the drying temperature is preferably -20 to 50°C, more preferably -20 to 35°C; the drying time is preferably 0.5 to 48h, more preferably 1 to 36h. In the present invention, the temperature of the normal pressure curing is preferably 30 to 80°C, more preferably 50 to 60°C; the time of the normal pressure curing is preferably 2 to 72 hours, more preferably 6 to 24 hours. In the present invention, the water absorption treatment is preferably soaked in deionized water. In the present invention, the temperature of the water absorption treatment is preferably room temperature; the time of the water absorption treatment is preferably 0.5 to 48 hours, more preferably 2 to 36 hours. In the present invention, the PVA absorbs water through the water absorption treatment, and can release water when under pressure, and can absorb water again to maintain its original state when the pressure is reduced, thereby increasing the elasticity and lubricity of the PVA hydrogel.
[0142] In the present invention, the hydrogel has a good porous structure, which is similar to the cartilage tissue structure in the human body. At the same time, the hydrogel has good compression performance, water absorption performance, good biocompatibility and weak antigenicity. It can be well combined with the original cartilage tissue in the human body or animal body, and improve the cell adhesion of the PVA hydrogel. The addition of PVA in the present invention can improve the biocompatibility of the resin ceramic composite material, and at the same time improve the toughness, and obtain a composite material with balanced hardness and toughness.
[0143] The present invention provides the use of the resin ceramic composite material described in the above technical solution or the resin ceramic composite material prepared by the preparation method described in the above technical solution in preparing biomedical materials. In the present invention, the biomedical material preferably includes a denture, an artificial eye or a bionic bone. In the present invention, the method of application preferably includes: processing the resin ceramic composite material to obtain a biomedical material. In the present invention, the processing method preferably includes turning.
[0144] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0145] In an embodiment of the present invention, the molecular weight of PMMA is 100,000-120,000.
[0146] Example 1 Preparation of ceramic skeleton
[0147] 1 μm albite is used as the main raw material, 5% PVA aqueous solution (the average molecular weight of PVA is 155000) is used as a binder, PEG (the molecular weight of PEG is 400) is used as a plasticizer, triammonium citrate is used as a dispersant, PMMA is used as a pore-forming agent, and deionized water is used as a medium, wherein the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate and deionized water is 100:12:0.4:0.7:86.9; three different casting slurries are prepared according to different contents and different particle sizes of PMMA, wherein the mass ratio of albite to PMMA in the first casting slurry is 90:5, and the particle size of PMMA in the first casting slurry is 2 μm; the mass ratio of albite to PMMA in the second casting slurry is 90:7, and the particle size of PMMA in the second casting slurry is 3 μm; the mass ratio of albite to PMMA in the third casting slurry is 90:9, and the particle size of PMMA in the third casting slurry is 4 μm;
[0148] According to the above raw material ratio, albite, PMMA, deionized water and triammonium citrate were ball-milled (the ball milling speed was 20 r / min) for 12 h, and then PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 20 r / min) for 8 h; the ball-milled slurry was vacuum-stirred for 1 h, and the bubbles were removed to obtain the first casting slurry, the second casting slurry and the third casting slurry respectively; the casting slurry without adding PMMA was prepared by the same method;
[0149] The above casting slurries were respectively cast, the scraper height was adjusted to 0.3 mm, the casting speed was 0.5 m / min, and a casting sheet with a thickness of 0.12 mm was obtained;
[0150] Each cast sheet is cut into square sheets of 210 mm × 210 mm by an automatic cutting machine, and then laminated by an automatic laminating machine. When laminating, from top to bottom, there are a cast sheet layer without PMMA added and a thickness of 6 mm, a cast sheet layer formed by the first cast slurry with a thickness of 6 mm, a cast sheet layer formed by the second cast slurry with a thickness of 6 mm, and a cast sheet layer formed by the third cast slurry with a thickness of 6 mm, wherein the cast sheet layer without PMMA is obtained by laminating multiple cast sheets without PMMA, and the first cast slurry is formed by The cast sheet layer is obtained by laminating a plurality of cast sheets formed by the first cast slurry, the cast sheet layer formed by the second cast slurry is obtained by laminating a plurality of cast sheets formed by the second cast slurry, and the cast sheet layer formed by the third cast slurry is obtained by laminating a plurality of cast sheets formed by the third cast slurry; the laminated sample is preliminarily pressed into a sample block with a thickness of 20 mm, and then hot-pressed under the conditions of warm isostatic pressing of 90 MPa and temperature of 40° C., with a holding time of 5 min, and a 200 mm×200 mm laminated sheet is obtained by cutting off four sides with a cutting machine;
[0151] The laminated sheet was cut into small pieces of 16 mm × 16 mm × 20 mm, placed in a high-temperature furnace, heated from room temperature to 290°C over 240 min, kept at 290°C for 60 min, heated to 410°C over 120 min, kept at 410°C for 1 h, heated to 1000°C over 240 min, kept at 1000°C for 5.0 h, and obtained as shown in the following figure. Fig.11 The ceramic skeleton shown has a connected pore structure, and its pore diameter gradually increases from top to bottom.
[0152] Example 2 Preparation of ceramic skeleton
[0153] 0.1 μm sodium aluminum silicate is used as the main raw material, 5% mass concentration of PVA aqueous solution (the average molecular weight of PVA is 155000) is used as a binder, PEG (the molecular weight of PEG is 400) is used as a plasticizer, triammonium citrate is used as a dispersant, PMMA is used as a pore-forming agent, and deionized water is used as a medium, wherein the mass ratio of sodium aluminum silicate, PVA aqueous solution, PEG, triammonium citrate and deionized water is 100:8:0.3:0.6:91.1; according to PMMA Three different casting slurries were prepared with different contents and different particle sizes, wherein the mass ratio of sodium aluminum silicate to PMMA in the first casting slurry was 90:10, and the particle size of PMMA in the first casting slurry was 30 μm; the mass ratio of sodium aluminum silicate to PMMA in the second casting slurry was 90:12, and the particle size of PMMA in the second casting slurry was 40 μm; the mass ratio of sodium aluminum silicate to PMMA in the third casting slurry was 90:14, and the particle size of PMMA in the third casting slurry was 50 μm;
[0154] According to the above raw material ratio, sodium aluminum silicate, PMMA, deionized water and triammonium citrate were ball-milled (the ball milling speed was 30 r / min) for 12 h, and then the PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 30 r / min) for 8 h; the ball-milled slurry was vacuum-stirred for 1 h, and the bubbles were removed to obtain the first casting slurry, the second casting slurry and the third casting slurry respectively;
[0155] The above casting slurries were respectively cast, the scraper height was adjusted to 0.35 mm, the casting speed was 0.3 m / min, and a casting sheet with a thickness of 0.15 mm was obtained;
[0156] Each cast sheet is cut into a square sheet of 210mm×210mm by an automatic cutting machine, and then laminated by an automatic laminating machine. When laminating, from top to bottom, there are cast sheet layers formed by a first cast slurry with a thickness of 8.1mm, a cast sheet layer formed by a third cast slurry with a thickness of 8.1mm, and a cast sheet layer formed by a second cast slurry with a thickness of 8.1mm, wherein the cast sheet layer formed by the first cast slurry is obtained by laminating a plurality of cast sheets formed by the first cast slurry, the cast sheet layer formed by the third cast slurry is obtained by laminating a plurality of cast sheets formed by the third cast slurry, and the cast sheet layer formed by the second cast slurry is obtained by laminating a plurality of cast sheets formed by the second cast slurry; the laminated sample is preliminarily pressurized into a sample block with a thickness of 20mm, and then hot-pressed under the conditions of warm isostatic pressing of 90MPa and a temperature of 40°C for a holding time of 5min, and a 200mm×200mm laminated sheet is obtained by cutting off the four sides by a cutting machine;
[0157] The laminated sheet was cut into small pieces of 16 mm × 16 mm × 20 mm, placed in a high-temperature furnace, heated from room temperature to 290°C over 240 min, kept at 290°C for 60 min, heated to 410°C over 120 min, kept at 410°C for 1 h, heated to 820°C over 200 min, kept at 820°C for 2.0 h, and obtained as shown in the following figure. Fig.15 The ceramic skeleton shown has a connected pore structure, and its pore size first increases and then decreases.
[0158] Example 3 Preparation of ceramic skeleton
[0159] 4 μm albite is used as the main raw material, 5% PVA aqueous solution (the average molecular weight of PVA is 155000) is used as a binder, PEG (the molecular weight of PEG is 400) is used as a plasticizer, triammonium citrate is used as a dispersant, PMMA is used as a pore-forming agent, and deionized water is used as a medium, wherein the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate and deionized water is 100:9:0.35:0.65:90; three different casting slurries are prepared according to different contents and different particle sizes of PMMA, wherein the mass ratio of albite to PMMA in the first casting slurry is 90:15, and the particle size of PMMA in the first casting slurry is 5 μm; the mass ratio of albite to PMMA in the second casting slurry is 90:18, and the particle size of PMMA in the second casting slurry is 25 μm; the mass ratio of albite to PMMA in the third casting slurry is 90:21, and the particle size of PMMA in the third casting slurry is 50 μm;
[0160] According to the above raw material ratio, albite, PMMA, deionized water and triammonium citrate were ball-milled (the ball milling speed was 20 r / min) for 12 h, and then PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 20 r / min) for 8 h; the ball-milled slurry was vacuum-stirred for 1 h, and the bubbles were removed to obtain the first casting slurry, the second casting slurry and the third casting slurry respectively;
[0161] The above casting slurries were respectively cast, the scraper height was adjusted to 0.35 mm, the casting speed was 0.3 m / min, and a casting sheet with a thickness of 0.15 mm was obtained;
[0162] Each cast sheet is cut into a square sheet of 210mm×210mm by an automatic cutting machine, and then laminated by an automatic laminating machine. When laminating, from top to bottom, there are cast sheets formed by a second cast slurry with a thickness of 6mm, a cast sheet formed by a first cast slurry with a thickness of 8mm, and a cast sheet formed by a third cast slurry with a thickness of 10mm, wherein the cast sheet formed by the second cast slurry is obtained by laminating a plurality of cast sheets formed by the second cast slurry, the cast sheet formed by the first cast slurry is obtained by laminating a plurality of cast sheets formed by the first cast slurry, and the cast sheet formed by the third cast slurry is obtained by laminating a plurality of cast sheets formed by the third cast slurry; the laminated sample is preliminarily pressurized into a sample block with a thickness of 20mm, and then hot-pressed under the conditions of warm isostatic pressing of 90MPa and 40°C for a holding time of 5min, and a 200mm×200mm laminated sheet is obtained by cutting off the four sides by a cutting machine;
[0163] The laminated sheet was cut into small pieces of 16 mm × 16 mm × 20 mm, placed in a high-temperature furnace, heated from room temperature to 290°C over 240 min, kept at 290°C for 60 min, heated to 410°C over 120 min, kept at 410°C for 1 h, heated to 1120°C over 270 min, kept at 1120°C for 1.5 h, and obtained as shown in the figure. Fig.10 The pore size shown first decreases and then increases, showing a ceramic skeleton with a connected pore structure.
[0164] Example 4 Preparation of ceramic skeleton
[0165] 1.5 μm albite is used as the main raw material, 5% PVA aqueous solution (the average molecular weight of PVA is 155000) is used as a binder, PEG (the molecular weight of PEG is 400) is used as a plasticizer, triammonium citrate is used as a dispersant, and deionized water is used as a medium, wherein the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate and deionized water is 100:12:0.4:0.7:86.9; four different casting slurries are prepared according to different types, different contents and different particle sizes of pore-forming agents, wherein the mass ratio of albite to pore-forming agent in casting slurry a is 90:20, the pore-forming agent is a mixture of PMMA and corn starch (the mass ratio of PMMA to corn starch is 1:1), and PMMA consists of PMMA with a particle size of 0.5 μm, PMMA with a particle size of 1 μm and PMMA with a particle size of 10 μm. The mass ratio of albite and pore former is 90:20 in the casting slurry b, the pore former is PMMA, and PMMA is obtained by mixing PMMA with a particle size of 5 μm, PMMA with a particle size of 10 μm and PMMA with a particle size of 25 μm in a mass ratio of 1:1:1; the mass ratio of albite and pore former in the casting slurry c is 90:10, the pore former is PMMA, and PMMA is obtained by mixing PMMA with a particle size of 10 μm, PMMA with a particle size of 20 μm and PMMA with a particle size of 45 μm in a mass ratio of 1:1:2; the mass ratio of albite and pore former in the casting slurry d is 90:5, the pore former is PMMA, and PMMA is obtained by mixing PMMA with a particle size of 20 μm, PMMA with a particle size of 25 μm and PMMA with a particle size of 50 μm in a mass ratio of 1:1:3;
[0166] According to the above raw material ratio, albite, pore former, deionized water and triammonium citrate were ball-milled (the ball milling speed was 20 r / min) for 12 h, and then PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 20 r / min) for 12 h; the ball-milled slurry was vacuum-stirred for 1 h, and after removing the bubbles inside, casting slurry a, casting slurry b, casting slurry c and casting slurry d were obtained respectively;
[0167] The above casting slurries were respectively cast, the scraper height was adjusted to 0.35 mm, the casting speed was 0.3 m / min, and a casting sheet with a thickness of 0.15 mm was obtained;
[0168] Each cast sheet is cut into a square sheet of 210 mm × 210 mm by an automatic cutting machine, and then laminated by an automatic laminating machine. When laminating, from top to bottom, there is a cast sheet layer formed by a casting slurry a with a thickness of 3 mm, a cast sheet layer formed by a casting slurry b with a thickness of 6 mm, a cast sheet layer formed by a casting slurry c with a thickness of 7 mm, and a cast sheet layer formed by a casting slurry d with a thickness of 8 mm, wherein the cast sheet layer formed by the casting slurry a is obtained by laminating a plurality of cast sheets formed by the casting slurry a, and the cast sheet layer formed by the casting slurry b is obtained by laminating a plurality of cast sheets formed by the casting slurry The cast sheet layer is obtained by laminating a plurality of cast sheets formed by cast slurries b, the cast sheet layer formed by cast slurry c is obtained by laminating a plurality of cast sheets formed by cast slurries c; the cast sheet layer formed by cast slurry d is obtained by laminating a plurality of cast sheets formed by cast slurries d; the laminated sample is preliminarily pressed into a sample block with a thickness of 20 mm, and then hot-pressed under the conditions of warm isostatic pressing at 90 MPa and a temperature of 40° C. for a holding time of 5 min, and a 200 mm×200 mm laminated sheet is obtained by cutting off the four sides with a cutting machine;
[0169] The laminated sheet was cut into small pieces of 16 mm × 16 mm × 20 mm, placed in a high-temperature furnace, heated from room temperature to 290°C over 240 min, kept at 290°C for 60 min, heated to 410°C over 120 min, kept at 410°C for 1 h, heated to 1030°C over 255 min, kept at 1030°C for 2.0 h, and obtained as shown in the following figure. Figure 1 The ceramic skeleton with a through-hole structure has a pore size that gradually increases from one end to the other end.
[0170] Example 5 Preparation of ceramic skeleton
[0171] 1.5 μm albite was used as the main raw material, 5% mass concentration of PVA aqueous solution (the average molecular weight of PVA was 155000) was used as a binder, PEG (the molecular weight of PEG was 400) was used as a plasticizer, triammonium citrate was used as a dispersant, PMMA was used as a pore-forming agent, and deionized water was used as a medium, wherein the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate and deionized water was 100:12:0.4:0.7:86.9; three different casting slurries were prepared according to different contents and different particle sizes of PMMA, wherein the mass ratio of albite to PMMA in casting slurry a was 90:15, and the mass ratio of PMMA to albite in casting slurry b was 90:15. A is obtained by mixing PMMA with a particle size of 0.5 μm, PMMA with a particle size of 1 μm and PMMA with a particle size of 10 μm in a mass ratio of 1:1:1; in the casting slurry b, the mass ratio of albite to PMMA is 90:21, and PMMA is obtained by mixing PMMA with a particle size of 5 μm, PMMA with a particle size of 10 μm and PMMA with a particle size of 25 μm in a mass ratio of 1:1:1; in the casting slurry c, the mass ratio of albite to PMMA is 90:18, and PMMA is obtained by mixing PMMA with a particle size of 10 μm, PMMA with a particle size of 20 μm and PMMA with a particle size of 45 μm in a mass ratio of 1:1:2;
[0172] According to the above raw material ratio, albite, PMMA, deionized water and triammonium citrate were ball-milled (the ball milling speed was 20 r / min) for 12 h, and then PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 20 r / min) for 8 h; the ball-milled slurry was vacuum-stirred for 1 h, and after removing the bubbles inside, casting slurry a, casting slurry b and casting slurry c were obtained respectively;
[0173] The above casting slurries were respectively cast, the scraper height was adjusted to 0.35 mm, the casting speed was 0.3 m / min, and a casting sheet with a thickness of 0.15 mm was obtained;
[0174] Cut each cast sheet into square sheets of 210 mm × 210 mm by an automatic cutting machine, and then laminate them by an automatic laminating machine. When laminating, the cast sheet layer formed by the cast slurry a with a thickness of 8 mm, the cast sheet layer formed by the cast slurry c with a thickness of 8 mm, and the cast sheet layer formed by the cast slurry b with a thickness of 8 mm are sequentially formed from top to bottom, wherein the cast sheet layer formed by the cast slurry a is obtained by laminating a plurality of cast sheets formed by the cast slurry a, the cast sheet layer formed by the cast slurry c is obtained by laminating a plurality of cast sheets formed by the cast slurry c, and the cast sheet layer formed by the cast slurry b is obtained by laminating a plurality of cast sheets formed by the cast slurry b; the laminated sample is preliminarily pressurized into a sample block with a thickness of 20 mm, and then hot-pressed under the conditions of warm isostatic pressing at 90 MPa and a temperature of 40° C., with a holding time of 5 min, and the four sides are cut off by a cutting machine to obtain a laminated sheet of 200 mm × 200 mm;
[0175] The laminated sheet was cut into small pieces of 16 mm × 16 mm × 20 mm, placed in a high-temperature furnace, heated from room temperature to 290°C over 240 min, kept at 290°C for 60 min, heated to 410°C over 120 min, kept at 410°C for 1 h, heated to 1050°C over 260 min, kept at 1050°C for 2.5 h, and obtained as shown in the following figure. Figure 3 The ceramic skeleton shown has a through-hole structure, and its pore diameter increases first and then decreases from one end to the other end.
[0176] Example 6 Preparation of ceramic skeleton
[0177] 1.8 μm albite is used as the main raw material, 5% mass concentration of PVA aqueous solution (the average molecular weight of PVA is 155000) is used as a binder, PEG (the molecular weight of PEG is 400) is used as a plasticizer, triammonium citrate is used as a dispersant, and deionized water is used as a medium, wherein the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate and deionized water is 100:12:0.4:0.7:86.9; according to the different types, contents and Four different casting slurries were prepared with the same particle size. In the casting slurry a, the mass ratio of albite to pore-forming agent was 90:15, the pore-forming agent was a mixture of PMMA and corn starch (the mass ratio of PMMA to corn starch was 1:1), and PMMA was obtained by mixing PMMA with a particle size of 0.5 μm, PMMA with a particle size of 1 μm, and PMMA with a particle size of 10 μm in a mass ratio of 1:1:1; in the casting slurry b, the mass ratio of albite to pore-forming agent was 90:15, the pore-forming agent was P MMA, PMMA is obtained by mixing PMMA with a particle size of 5 μm, PMMA with a particle size of 10 μm and PMMA with a particle size of 25 μm in a mass ratio of 1:1:1; the mass ratio of albite to pore-forming agent in casting slurry c is 90:15, the pore-forming agent is PMMA, and PMMA is obtained by mixing PMMA with a particle size of 10 μm, PMMA with a particle size of 20 μm and PMMA with a particle size of 45 μm in a mass ratio of 1:1:2; the mass ratio of albite to pore-forming agent in casting slurry d is 90:15, the pore-forming agent is PMMA, and PMMA is obtained by mixing PMMA with a particle size of 10 μm, PMMA with a particle size of 20 μm and PMMA with a particle size of 45 μm in a mass ratio of 1:1:2. The mass ratio of albite to the pore-forming agent is 90:15, the pore-forming agent is PMMA, and PMMA is obtained by mixing PMMA with a particle size of 10 μm, PMMA with a particle size of 20 μm, and PMMA with a particle size of 45 μm in a mass ratio of 1:1:3; the mass ratio of albite to the pore-forming agent in the casting slurry e is 90:15, the pore-forming agent is PMMA, and PMMA is obtained by mixing PMMA with a particle size of 10 μm, PMMA with a particle size of 25 μm, and PMMA with a particle size of 50 μm in a mass ratio of 1:1:2;
[0178] According to the above raw material ratio, albite, pore-forming agent, deionized water and triammonium citrate were ball-milled (the ball milling speed was 20 r / min) for 12 h, and then PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 20 r / min) for 8 h; the ball-milled slurry was vacuum-stirred for 1 h, and after removing the bubbles inside, casting slurry a, casting slurry b, casting slurry c, casting slurry d and casting slurry e were obtained respectively;
[0179] The above casting slurries were respectively cast, the scraper height was adjusted to 0.35 mm, the casting speed was 0.3 m / min, and a casting sheet with a thickness of 0.15 mm was obtained;
[0180] Each cast sheet is cut into a square sheet of 210 mm × 210 mm by an automatic cutting machine, and then laminated by an automatic laminating machine. During lamination, the middle layer is a cast sheet layer formed by the casting slurry a, and the upper and lower layers next to the middle layer are cast sheets formed by the casting slurry b. The outer side of the cast sheet layer formed by the casting slurry b is a cast sheet layer formed by the casting slurry c, and then outwards are the cast sheet layer formed by the casting slurry d and the cast sheet layer formed by the casting slurry e, a total of 9 layers, the thickness of the middle layer is 4 mm, and the thickness of each of the remaining layers is 2.5 mm, among which the cast sheet layer formed by the casting slurry a is composed of a plurality of cast sheets formed by the casting slurry a. The cast sheet layer formed by the casting slurry b is obtained by laminating a plurality of cast sheets formed by the casting slurries b, the cast sheet layer formed by the casting slurry c is obtained by laminating a plurality of cast sheets formed by the casting slurries c, the cast sheet layer formed by the casting slurry d is obtained by laminating a plurality of cast sheets formed by the casting slurries d, and the cast sheet layer formed by the casting slurry e is obtained by laminating a plurality of cast sheets formed by the casting slurries e; the laminated sample is preliminarily pressurized into a sample block with a thickness of 20 mm, and then hot-pressed under the conditions of warm isostatic pressing of 90 MPa and temperature of 40° C., with a holding time of 5 min, and a 200 mm×200 mm laminated sheet is obtained by cutting off the four sides with a cutting machine;
[0181] The laminated sheet was cut into small pieces of 16 mm × 16 mm × 20 mm, placed in a high-temperature furnace, heated from room temperature to 290°C over 240 min, kept at 290°C for 60 min, heated to 410°C over 120 min, kept at 410°C for 1 h, heated to 1080°C over 270 min, kept at 1080°C for 3.5 h, and obtained as shown in the following figure. Figure 2 The ceramic skeleton shown has a through-hole structure, and its pore size decreases first and then increases.
[0182] Example 7 Preparation of Ceramic Skeleton
[0183] 5.0 μm albite is used as the main raw material, 10% mass concentration of PVA aqueous solution (the average molecular weight of PVA is 155000) is used as a binder, PEG (the molecular weight of PEG is 400) is used as a plasticizer, triammonium citrate is used as a dispersant, PMMA is used as a pore-forming agent, and deionized water is used as a medium; three different casting slurries are prepared according to the different contents of each component, wherein the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate, deionized water and PMMA in ceramic slurry a is 100:12:0.4:0.7:50:5, and PMMA is a mixture of PMMA with a particle size of 50 μm, PMMA with a particle size of 80 μm and PMMA with a particle size of 100 μm in a mass ratio of 1:1:1 The mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate, deionized water and PMMA in ceramic slurry b is 100:12:0.4:0.7:55:10, and PMMA is obtained by mixing PMMA with a particle size of 100 μm, PMMA with a particle size of 300 μm and PMMA with a particle size of 500 μm in a mass ratio of 1:1:1; the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate, deionized water and PMMA in ceramic slurry c is 100:12:0.4:0.7:60:15, and PMMA is obtained by mixing PMMA with a particle size of 500 μm, PMMA with a particle size of 700 μm and PMMA with a particle size of 1000 μm in a mass ratio of 1:1:1;
[0184] According to the above raw material ratio, albite, PMMA, deionized water and ammonium citrate were ball-milled (the ball milling speed was 20 r / min) for 12 h, and then PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 20 r / min) for 8 h; the ball-milled slurry was vacuum-stirred for 1 h, and after removing the bubbles inside, ceramic slurry a, ceramic slurry b and ceramic slurry c were obtained respectively;
[0185] Ceramic slurry a is introduced into mold 1 and frozen in a -20°C freezer for 1 hour, and a first frozen block is obtained after the freezing is completed; the first frozen block is placed in mold 2, and three ejector pins are provided at the bottom of mold 2, so that the first frozen block is suspended in mold 2, and then ceramic slurry b is poured into mold 2 and covers the first frozen block, and mold 2 is placed in a -20°C freezer and frozen again for 1 hour to obtain a second frozen block;
[0186] The second frozen block is placed in the mold 3. There are three ejector pins at the bottom of the mold 3, which can allow the second frozen block to be suspended in the mold 3. Then, the ceramic slurry c is poured into the mold 3 and covers the second frozen block. The mold 3 is placed in a -80°C freezer and frozen again for 1 hour to obtain a third frozen block.
[0187] The third frozen block was placed in a vacuum freeze drying box, and dried at 50Pa and 5°C for 6 hours to obtain a dried sample block; the dried sample block was placed in a high-temperature furnace, and the temperature was raised from room temperature to 290°C after 240 minutes, and kept at 290°C for 60 minutes, and then the temperature was raised to 410°C after 120 minutes, and kept at 410°C for 1 hour, and then the temperature was raised to 1200°C after 300 minutes, and kept at 1200°C for 1.0 hour, and the following was obtained: Fig.13 The ceramic skeleton shown has a three-dimensional through-hole structure, in which the pore size gradually increases from the inside to the surroundings.
[0188] Example 8 Preparation of Ceramic Framework
[0189] 3.0 μm albite is used as the main raw material, 12% mass concentration of PVA aqueous solution (the average molecular weight of PVA is 155000) is used as a binder, PEG (the molecular weight of PEG is 400) is used as a plasticizer, triammonium citrate is used as a dispersant, PMMA is used as a pore-forming agent, and deionized water is used as a medium; three different casting slurries are prepared according to the different contents of each component, wherein the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate, deionized water and PMMA in ceramic slurry a is 100:12:0.4:0.7:50:5, and PMMA is composed of PMMA with a particle size of 50 μm, PMMA with a particle size of 80 μm and PMMA with a particle size of 100 μm in a mass ratio of 1:2:1 Mixed; the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate, deionized water and PMMA in ceramic slurry b is 100:12:0.4:0.7:55:10, and PMMA is obtained by mixing PMMA with a particle size of 70 μm, PMMA with a particle size of 100 μm and PMMA with a particle size of 150 μm in a mass ratio of 1:2:1; the mass ratio of albite, PVA aqueous solution, PEG, triammonium citrate, deionized water and PMMA in ceramic slurry c is 100:12:0.4:0.7:60:15, and PMMA is obtained by mixing PMMA with a particle size of 100 μm, PMMA with a particle size of 150 μm and PMMA with a particle size of 200 μm in a mass ratio of 1:2:1;
[0190] According to the above raw material ratio, albite, PMMA, deionized water and ammonium citrate were ball-milled (the ball milling speed was 20 r / min) for 12 h, and then PVA aqueous solution and PEG were added for secondary ball-milling (the ball milling speed was 20 r / min) for 8 h; the ball-milled slurry was vacuum-stirred for 1 h, and after removing the bubbles inside, ceramic slurry a, ceramic slurry b and ceramic slurry c were obtained respectively;
[0191] The ceramic slurry a is introduced into the mold 1 and frozen in a -30°C freezer for 1 hour, and a first frozen block is obtained after the freezing is completed; the first frozen block is placed in the mold 2b, and then the ceramic slurry b is poured into the mold 2b and covered with the first frozen block, and the mold 2b is placed in a -30°C freezer and frozen again for 1 hour to obtain a second frozen block;
[0192] The second frozen block is placed in the mold 3c, and then the ceramic slurry c is poured into the mold 3c to cover the second frozen block, and the mold 3c is placed in a -30°C freezer and frozen again for 1 hour to obtain a third frozen block;
[0193] The third frozen block was placed in a 5°C vacuum freeze drying box and dried at 50Pa for 4 hours to obtain a dried sample block; the dried sample block was placed in a high-temperature furnace, heated from room temperature to 290°C over 240 minutes, kept at 290°C for 60 minutes, heated to 410°C over 120 minutes, kept at 410°C for 1 hour, heated to 1100°C over 280 minutes, kept at 1100°C for 4.5 hours, and obtained as shown in the following figure. Fig.14 The ceramic skeleton shown has a divergent through-hole structure with pore sizes gradually increasing from a starting position.
[0194] Example 9 Preparation of Ceramic Framework
[0195] 5 μm albite and 100 nm sodium aluminum silicate are used as main raw materials, with a mass ratio of 6:4; 3% mass concentration PVA aqueous solution is used as a binder, with a mass ratio of 1:10 to the main raw material; anhydrous ethanol is used as a solvent, with a mass ratio of 3:2 to the main raw material;
[0196] The main raw material, the binder and the solvent were wet-milled at a speed of 26 revolutions per minute for a ball-milling time of 3 hours to obtain a ball-milled material;
[0197] Drying the ball mill material at 55° C. for 12 hours to obtain dry powder;
[0198] The dry powder is passed through a 100-mesh sieve, and then the sieved material is dry-pressed at a pressure of 10 MPa for 50 seconds to obtain a dry pressed block;
[0199] The dry pressed block is isostatically pressed at 230 MPa for 3 minutes to obtain a green body;
[0200] The green body is placed in a high-temperature furnace, and the temperature is raised from room temperature to 290°C after 240 minutes, kept at 290°C for 60 minutes, raised to 410°C after 120 minutes, kept at 410°C for 1 hour, raised to 890°C after 180 minutes, and kept at 890°C for 4 hours to obtain a ceramic skeleton, whose pore structure distribution is relatively uniform, the pore sizes are relatively close, and there is no obvious change trend.
[0201] Example 10 Preparation of ceramic skeleton
[0202] 3.5 μm albite is used as the main raw material, 2 μm PMMA and potato flour are used as pore formers, and hydroxypropyl methylcellulose is used as a binder; the mass ratio of the pore former to the main raw material is 1:10; the potato flour is the undersize obtained by passing through a 180-mesh sieve, wherein the mass ratio of PMMA to potato flour is 1:1; the mass ratio of hydroxypropyl methylcellulose to the main raw material is 1:20;
[0203] Using a mixer, albite, PMMA, potato flour and hydroxypropyl methylcellulose are dry-mixed according to a proportion to obtain a mixture;
[0204] The mixed material, glycerin, water and 3% mass concentration of PVA aqueous solution are added into a kneader for kneading to obtain a kneaded material; the mass ratio of glycerin to the main raw material is 1.5:100; the mass ratio of water to the main raw material is 26.5:100; the mass ratio of PVA aqueous solution to the main raw material is 1:100; the kneader speed is 15 rpm;
[0205] The kneaded material was aged for 12 hours and then kneaded using a kneading machine to obtain a mud block; the extrusion speed of the kneading machine was 80 cm / min;
[0206] The mud block is segmented by a mud segmentation machine to obtain mud segments; the mud segmentation machine has an extrusion speed of 30 cm / min;
[0207] The clay segments are placed in an extrusion molding machine for extrusion and cutting to obtain wet blanks; the extrusion speed of the extrusion molding machine is 50 cm / min;
[0208] The wet billet is subjected to microwave drying to obtain a dry billet; the microwave power of the microwave drying is 3 kW, and the microwave drying time is 65 s;
[0209] The dry blank was placed in a high-temperature furnace, heated from room temperature to 290°C over 240 minutes, kept at 290°C for 60 minutes, heated to 410°C over 120 minutes, kept at 410°C for 1 hour, heated to 1100°C over 280 minutes, and kept at 1100°C for 3 hours to obtain the following Figure 8 The ceramic skeleton shown has a three-dimensional through-pore structure.
[0210] Examples 11-20 Preparation of resin ceramic composite materials
[0211] Preparation of resin precursor solution:
[0212] Bis-GMA, UDMA, TEGDMA and BPO were mixed in the proportions shown in Table 1 to obtain a resin precursor solution. In Example 19, the mass fraction of BPO in the resin precursor solution was 0.1%, and in the remaining examples, the mass fraction of BPO in the resin precursor solution was 0.55%.
[0213] Ceramic skeleton modification:
[0214] The ceramic skeleton prepared in the above embodiment was immersed in the silane modification liquid shown in Table 1, modified at room temperature for 24 hours, and then modified at 60° C. for 1.5 hours to obtain a modified ceramic skeleton.
[0215] Preparation of resin ceramic composite materials:
[0216] The modified ceramic skeleton was immersed in a resin precursor solution and vacuum impregnated at room temperature for 36 h at a pressure of 500 Pa. After impregnation, the resin was cured in a warm isostatic press (the curing pressure, temperature and time are shown in Table 1) to obtain a resin-ceramic composite material.
[0217] Table 1 Conditions for preparing resin ceramic composites
[0218]
[0219]
[0220] Example 21 Preparation of resin ceramic composite material
[0221] Preparation of PVA aqueous solution:
[0222] Weigh 85g of deionized water in a beaker, add 15g of PVA (average molecular weight 175000) into the beaker while stirring, and heat and stir at 90°C for 4h to obtain a viscous PVA aqueous solution;
[0223] Preparation of resin precursor solution:
[0224] Mix Bis-GMA, UDMA, TEGDMA and BPO to obtain a mixed solution; wherein the mass ratio of Bis-GMA, UDMA and TEGDMA is 1:1:2, and the mass fraction of BPO in the mixed solution is 0.55%; fully stir and mix the mixed solution and the PVA aqueous solution at a volume ratio of 1:10 to obtain a resin precursor solution;
[0225] Ceramic skeleton modification:
[0226] The ceramic skeleton prepared in Example 8 was immersed in a silane modification solution (the mass ratio of anhydrous ethanol, distilled water, acetic acid and KH570 was 1:1:0.009:0.01), modified at room temperature for 24 hours, and then modified at 60°C for 1.5 hours to obtain a modified ceramic skeleton.
[0227] Preparation of resin-ceramic composite materials
[0228] The modified ceramic skeleton is immersed in the prepared resin precursor solution, and vacuum impregnation is performed at room temperature. The vacuum impregnation pressure is 1000 Pa and the vacuum impregnation time is 24 hours to obtain an impregnated ceramic skeleton;
[0229] The impregnated ceramic skeleton was frozen at -20°C for 12 hours, then thawed at room temperature, and the freezing and thawing were repeated twice. Then, vacuum drying was performed at 50Pa pressure and 5°C for 2 hours, and resin curing was performed at 50°C for 6 hours. The cured sample was placed in deionized water and soaked at room temperature and pressure for 2 hours to obtain a resin ceramic composite material.
[0230] The resin-ceramic composite material prepared in this embodiment has high hardness and strength. The resin is distributed in the PVA hydrogel and is firmly bonded with the ceramic skeleton.
[0231] Comparative Example 1
[0232] The preparation method is basically the same as that of Example 12, except that PMMA is not added, and the pore size distribution of the prepared ceramic skeleton is relatively uniform, with only a single pore structure.
[0233] Test Case
[0234] The properties of the resin ceramic composite materials prepared in Examples 11 to 20 and Comparative Example 1 are shown in Table 2. The testing standard for hardness in Table 2 is GB / T 4340.1-2009, the testing standard for fracture toughness is GB30367-2013, and the testing standard for flexural strength is GB 30367-2013. The properties of the resin ceramic composite material prepared in Example 21 are shown in Table 3. The testing standard for tensile strength in Table 3 is GB / T10654-2001, the testing standard for compression modulus is GB / T 1041-2008, and the testing standard for cytotoxicity grade is GB / T 16886.5-2017.
[0235] Table 2 Properties of the resin ceramic composite materials prepared in Examples 11 to 20 and Comparative Example 1
[0236]
[0237] Table 3 Performance comparison of the resin ceramic composite material prepared in Example 21 and human cartilage
[0238] project Tensile strength(MPa) Compression modulus (MPa) Cytotoxicity level Embodiment 21 15.2 5.7 0 Human cartilage 1~13.9 4 0
[0239] It can be seen from Table 2 that the density, strength and toughness of the resin-ceramic composite material are related to the pore-forming agent content. The higher the pore-forming agent content and the higher the porosity, the more resin can penetrate, so the overall density will decrease, the toughness will increase, and the strength will first increase and then decrease. In addition, for the same porosity, the smaller the pore size, the less conducive it is to resin penetration, so the strength and toughness will decrease. Therefore, by adjusting different pore sizes and porosities, resin-ceramic composite materials with different mechanical properties can be obtained, which can be used in different scenarios to meet different needs.
[0240] As can be seen from Table 3, the PVA hydrogel resin ceramic composite material in Example 21 is close to human cartilage in terms of performance, and has similar stretchability and compressibility as cartilage, good elasticity and lubricity, and is qualified in the cytotoxicity test, and can be used as a substitute for human cartilage. In addition, by selecting raw materials with different particle sizes with good biocompatibility, adjusting the particle size and content of the pore-forming agent, and adjusting the water absorption of the PVA hydrogel, a porous structure and mechanical properties close to those of human bones can be obtained. Materials and porous structures with good biocompatibility are conducive to cell attachment and tissue repair, and can be used as human bionic bone materials.
[0241] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A ceramic skeleton, It is characterized in that The ceramic skeleton has a porous structure; The porous structure includes one or more of a connected pore structure and a through-pore structure; The interconnected hole structure is formed by a plurality of holes being interconnected; The through hole structure includes one or more of a unidirectional through hole structure and a divergent through hole structure.
2. The ceramic skeleton according to claim 1, It is characterized in that The holes in the interconnected hole structure are regular and / or irregular holes.
3. The ceramic skeleton according to claim 1, It is characterized in that The apertures of the holes in the interconnected hole structure increase sequentially from one end to the other, or the apertures of the holes increase first and then decrease from one end to the other, or the apertures of the holes decrease first and then increase from one end to the other.
4. The ceramic skeleton according to claim 1 or 3, It is characterized in that The pore diameter range of the holes in the interconnected pore structure is independently less than 1000 μm.
5. The ceramic skeleton according to claim 1, It is characterized in that The one-way through hole structure is composed of a plurality of through holes extending from one end to the other end.
6. The ceramic skeleton according to claim 1, It is characterized in that The divergent through-hole structure comprises a plurality of through-holes which diverge from a starting position inside the ceramic framework to the surrounding areas.
7. The ceramic skeleton according to claim 1, It is characterized in that The divergent through-hole structure includes a three-dimensional through-hole structure; The three-dimensional through hole structure is composed of a plurality of three-dimensional through holes penetrating upward, downward, leftward, rightward, and rearward.
8. The ceramic skeleton according to claim 1, It is characterized in that The aperture of each through hole in the one-way through hole structure increases independently from one end to the other, or the aperture of each through hole increases independently from one end to the other and then decreases, or the aperture of each through hole decreases independently from one end to the other and then increases.
9. The ceramic skeleton according to claim 1 or 8, It is characterized in that The aperture range of each through hole in the one-way through hole structure is independently less than 1000 μm.
10. The ceramic skeleton according to claim 1, It is characterized in that The aperture of each through hole in the divergent through hole structure increases gradually from a starting position to the surroundings to form a trumpet shape, or the aperture of each through hole decreases gradually from a starting position to the surroundings, or the aperture of each through hole increases first and then decreases from a starting position to the surroundings, or the aperture of each through hole decreases first and then increases from a starting position to the surroundings.
11. The ceramic skeleton according to claim 1 or 10, It is characterized in that The aperture range of each through hole in the divergent through hole structure is independently less than 1000 μm.
12. The ceramic skeleton according to claim 7, It is characterized in that The aperture of each three-dimensional through hole in the three-dimensional through hole structure increases gradually from the middle to the surroundings to form a trumpet shape, or the aperture of each three-dimensional through hole decreases gradually from the middle to the surroundings, or the aperture of each three-dimensional through hole increases first and then decreases from the middle to the surroundings, or the aperture of each three-dimensional through hole decreases first and then increases from the middle to the surroundings.
13. The ceramic skeleton according to claim 7 or 12, It is characterized in that The pore size range of each three-dimensional through-hole in the three-dimensional through-hole structure is independently less than 1000 μm.
14. A method for preparing the ceramic skeleton according to any one of claims 1 to 13, The following steps are involved: Mixing a main raw material, a binder and a solvent to obtain a slurry; the main raw material includes one or more of a bio-inert ceramic material and a bio-active ceramic material; Casting the slurry to obtain a cast sheet; laminating the cast sheet to obtain a laminated sheet; The laminated sheets are sintered to obtain a ceramic skeleton.
15. A method for preparing the ceramic skeleton according to any one of claims 1 to 13, The following steps are involved: Mixing a main raw material and a solvent to obtain a ceramic slurry; the main raw material includes one or more of a bio-inert ceramic material and a bio-active ceramic material; Freezing the ceramic slurry to obtain a frozen block; Drying the frozen block to obtain a dried sample block; The dried sample is sintered to obtain a ceramic skeleton.
16. A method for preparing the ceramic skeleton according to any one of claims 1 to 13, The following steps are involved: Mixing main raw materials to obtain ceramic powder; the main raw materials include one or more of biologically inert ceramic materials and biologically active ceramic materials; Dry pressing and / or isostatic pressing the ceramic powder to obtain a green body; The green body is sintered to obtain a ceramic skeleton.
17. A method for preparing the ceramic skeleton according to any one of claims 1 to 13, The following steps are involved: Mixing main raw materials to obtain a mixture; the main raw materials include one or more of a bio-inert ceramic material and a bio-active ceramic material; kneading the mixed material, the binder and the solvent to obtain a kneaded material; The kneaded material is aged and then kneaded to obtain a kneaded mud block; The conditioned clay block is segmented to obtain clay segments; Extruding the mud segment to obtain a wet blank; Drying the wet blank to obtain a dry blank; The dry blank is sintered to obtain a ceramic skeleton.
18. Use of the ceramic skeleton according to any one of claims 1 to 13 or the ceramic skeleton prepared by the preparation method according to any one of claims 14 to 17 in the preparation of biomedical materials.
19. The use according to claim 18, It is characterized in that The biomedical material includes artificial teeth, artificial eyes or bionic bones.
20. A resin ceramic composite material, It is characterized in that It comprises a ceramic skeleton and a resin filled in the porous structure of the ceramic skeleton; the ceramic skeleton is the ceramic skeleton described in any one of claims 1 to 13 or a ceramic skeleton prepared by the preparation method described in any one of claims 14 to 17.
21. The resin-ceramic composite material according to claim 20, It is characterized in that The raw materials for preparing the resin include one or more of monofunctional acrylate and multifunctional acrylate.
22. A method for preparing the resin-ceramic composite material according to any one of claims 20 to 21, The following steps are involved: The ceramic skeleton is immersed in a resin precursor solution and solidified to obtain a resin-ceramic composite material.
23. The preparation method according to claim 22, It is characterized in that The curing pressure is 0.1-500 MPa; the curing temperature is 10-180° C.; and the curing heat preservation and pressure holding time is 1 min-48 h.
24. Use of the resin-ceramic composite material according to any one of claims 20 to 21 or the resin-ceramic composite material prepared by the preparation method according to any one of claims 22 to 23 in the preparation of biomedical materials.
25. The use according to claim 24, It is characterized in that The biomedical material includes artificial teeth, artificial eyes or bionic bones.
Citation Information
Patent Citations
Three-dimensional connected honeycomb porous calcium phosphate ceramic artificial bone material and preparation method thereof
CN106518143A
Silicon nitride-resin double continuous phase composite ceramic material and preparation method and application thereof
CN107056319A
Silicon nitride-resin bicontinuous phase composite ceramic material, and manufacturing method and application thereof
CN111302823A
Porous ceramic atomizing core, preparation method thereof and electronic cigarette
CN112759414A
Composite material bionic false tooth and manufacturing method thereof
CN114617656A