Solid-phase synthesis method of high-purity gallium oxalate

The solid phase synthesis method addresses the environmental and health risks of gallium oxalate production by eliminating waste liquids and enhancing purity and conversion rates through controlled mixing and reaction processes.

CN119059899APending Publication Date: 2024-12-03YANGZHOU NINGDA NOBLE METAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410965256.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing methods for synthesizing high-purity gallium oxalate generate significant gallium-containing waste liquids, posing environmental and health risks due to long-term exposure.

Method used

A solid phase synthesis method involving grinding gallium-containing metal sources and oxalic acid, mixing with a low eutectic solvent, and reacting under controlled conditions to produce high-purity gallium oxalate without generating waste liquids.

Benefits of technology

The method reduces environmental impact and health hazards by eliminating waste liquids while improving conversion rates and purity of gallium oxalate production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059899A_ABST
    Figure CN119059899A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fine chemical synthesis, in particular to a solid-phase synthesis method of high-purity gallium oxalate, which comprises the following steps: respectively grinding a gallium-containing metal source and oxalic acid to obtain gallium-containing metal source powder and oxalic acid powder; mixing the ground gallium-containing metal source powder and oxalic acid powder to obtain a first mixture; adding the eutectic solvent into the first mixture and mixing to obtain a second mixture; transferring the second mixture into a reactor, carrying out temperature programming, and carrying out full reaction in an inert atmosphere; and cooling and grinding the obtained reaction product to obtain the high-purity gallium oxalate. According to the method, equipment and operation conditions are simple, gallium-containing waste liquid is not generated in the whole synthesis process, the method is green and environmentally friendly, harm to human bodies and the ecological environment can be reduced, and the conversion rate and purity of gallium oxalate can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fine chemical synthesis, in particular to a solid phase synthesis method of high-purity gallium oxalate. Background Art

[0002] Given the unique physical and chemical properties of gallium, gallium oxalate plays a key role in the electronics industry, especially in the precision preparation of semiconductor materials. It can provide a high-purity source of gallium atoms, which is indispensable for ensuring that semiconductor materials (such as silicon wafers) meet quality standards.

[0003] After searching, the invention patent with publication number CN116328694B discloses a high-purity gallium oxalate preparation device for preparing high-purity gallium oxalate. In the present invention, gallium oxalate is synthesized by reaction in a solution, which will produce a large amount of gallium-containing waste liquid. Long-term exposure of gallium-containing solution to the environment will not only cause certain damage to human skin, respiratory system, kidneys, etc., but also pollute the soil and water, affecting the ecological environment. In view of this, we propose a solid-phase synthesis method for high-purity gallium oxalate. Summary of the invention

[0004] The purpose of the present invention is to provide a solid phase synthesis method of high-purity gallium oxalate, so as to reduce the generation of gallium-containing waste liquid, improve the conversion rate of gallium oxalate, and reduce the impact on human body and ecological environment.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A solid phase synthesis method for high-purity gallium oxalate comprises the following steps:

[0007] S1, grinding the gallium-containing metal source and oxalic acid respectively to obtain gallium-containing metal source powder and oxalic acid powder;

[0008] S2, mixing the gallium-containing metal source powder and the oxalic acid powder ground in step S1 to obtain a first mixture;

[0009] S3, adding a deep eutectic solvent to the first mixture and mixing to obtain a second mixture;

[0010] S4, transferring the second mixture to a reactor, raising the temperature by a program, and reacting the mixture fully under an inert atmosphere;

[0011] S5. The obtained reaction product is cooled and then ground to obtain high-purity gallium oxalate.

[0012] Preferably, the gallium-containing metal source includes any one of gallium hydroxide and gallium oxyhydroxide.

[0013] Preferably, the particle size of the gallium-containing metal source powder and the oxalic acid powder is less than 1 μm.

[0014] Preferably, the low eutectic solvent is a mixture of choline chloride and oxalic acid, and the molar ratio of choline chloride to oxalic acid is 1:1 to 4, such as 1:1, 1:2, 1:3, 1:4, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] Preferably, the molar ratio of the gallium-containing metal source to oxalic acid is 1:1, and the molar ratio of the gallium-containing metal source to the low eutectic solvent is 1:0.02-0.2, such as 1:0.02, 1:0.05, 1:0.1, 1:0.2, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the mixing method is high-energy ball milling.

[0017] Preferably, the rotation speed of the high energy ball mill in step S2 is 600-800 rpm, such as 600 rpm, 650 rpm, 700 rpm, 800 rpm, etc., and the time of the high energy ball mill is 10-30 min, such as 10 min, 15 min, 20 min, 30 min, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0018] In step S3, the rotation speed of the high energy ball mill is 800-1000 rpm, such as 800 rpm, 850 rpm, 900 rpm, 1000 rpm, etc., and the time of the high energy ball mill is 30-60 min, such as 30 min, 40 min, 50 min, 60 min, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the temperature in the reactor is 160-180°C, such as 160°C, 170°C, 175°C, 180°C, etc., the heating rate is 5-15°C / min, such as 5°C / min, 10°C / min, 12°C / min, 15°C / min, etc., and the reaction time is 2-20h, such as 2h, 5h, 10h, 20h, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the inert atmosphere is any one of nitrogen, argon and helium, and the gas flow rate is 10 to 50 cc / min, such as 10 cc / min, 20 cc / min, 40 cc / min, 50 cc / min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The solid phase synthesis method of high-purity gallium oxalate synthesizes gallium oxalate by mixing and grinding a gallium-containing metal source, oxalic acid, and a low eutectic solvent, and drying and dehydrating the same. It does not require complicated equipment and operating conditions, and the entire synthesis process does not produce gallium-containing waste liquid. It is green and environmentally friendly, and can reduce harm to the human body and the ecological environment.

[0023] 2. The solid phase synthesis method of high-purity gallium oxalate improves the conversion rate and purity of gallium oxalate by adding a low eutectic solvent and mixing and grinding with a gallium-containing metal source and oxalic acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a flow chart of the solid phase synthesis method of high-purity gallium oxalate. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] A solid phase synthesis method for high-purity gallium oxalate comprises the following steps:

[0028] S1, grinding gallium hydroxide and oxalic acid, respectively, wherein the molar ratio of the gallium-containing metal source to oxalic acid is 1:1, to obtain gallium-containing metal source powder and oxalic acid powder, wherein the particle size of the gallium-containing metal source powder and oxalic acid powder is less than 1 μm;

[0029] S2, mixing the gallium-containing metal source powder and the oxalic acid powder ground in step S1, the mixing method is high-energy ball milling, the speed of the high-energy ball milling is 600 rpm, the time of the high-energy ball milling is 10 minutes, to obtain a first mixture;

[0030] S3, adding a low eutectic solvent to the first mixture for mixing, wherein the molar ratio of the gallium-containing metal source to the low eutectic solvent is 1:0.02, the low eutectic solvent is a mixture of choline chloride and oxalic acid, the molar ratio of choline chloride to oxalic acid is 1:1, the mixing method is high-energy ball milling, the rotation speed of the high-energy ball milling is 800 rpm, and the time of the high-energy ball milling is 30 minutes, to obtain a second mixture;

[0031] S4, transferring the second mixture to a reactor, wherein the temperature in the reactor is 160°C, the temperature is programmed, the heating rate is 5°C / min, the reaction is fully carried out under a nitrogen atmosphere, the gas flow rate is 10cc / min, and the reaction time is 2h;

[0032] S5. The obtained reaction product is cooled and then ground to obtain high-purity gallium oxalate.

[0033] In this embodiment, the conversion rate of gallium oxalate is 99.5%, and the purity of gallium oxalate is 99.92%.

[0034] Example 2

[0035] A solid phase synthesis method for high-purity gallium oxalate comprises the following steps:

[0036] S1, grinding gallium hydroxide and oxalic acid, respectively, wherein the molar ratio of the gallium-containing metal source to oxalic acid is 1:1, to obtain gallium-containing metal source powder and oxalic acid powder, wherein the particle size of the gallium-containing metal source powder and oxalic acid powder is less than 1 μm;

[0037] S2, mixing the gallium-containing metal source powder and the oxalic acid powder ground in step S1, the mixing method is high-energy ball milling, the rotation speed of the high-energy ball milling is 650 rpm, and the time of the high-energy ball milling is 15 minutes, to obtain a first mixture;

[0038] S3, adding a low eutectic solvent to the first mixture, wherein the molar ratio of the gallium-containing metal source to the low eutectic solvent is 1:0.05, the low eutectic solvent is a mixture of choline chloride and oxalic acid, the molar ratio of choline chloride to oxalic acid is 1:2, the mixing method is high-energy ball milling, the rotation speed of the high-energy ball milling is 850 rpm, and the time of the high-energy ball milling is 40 min, to obtain a second mixture;

[0039] S4, transferring the second mixture to a reactor, wherein the temperature in the reactor is 170°C, the temperature is programmed, the heating rate is 10°C / min, the mixture is fully reacted under an argon atmosphere, the gas flow rate is 20cc / min, and the reaction time is 5h;

[0040] S5. The obtained reaction product is cooled and then ground to obtain high-purity gallium oxalate.

[0041] In this embodiment, the conversion rate of gallium oxalate is 99.6%, and the purity of gallium oxalate is 99.94%.

[0042] Example 3

[0043] A solid phase synthesis method for high-purity gallium oxalate comprises the following steps:

[0044] S1, grinding gallium-containing metal source gallium oxyhydroxide and oxalic acid respectively, wherein the molar ratio of the gallium-containing metal source to oxalic acid is 1:1, to obtain gallium-containing metal source powder and oxalic acid powder, wherein the particle size of the gallium-containing metal source powder and oxalic acid powder is less than 1 μm;

[0045] S2, mixing the gallium-containing metal source powder and the oxalic acid powder ground in step S1, the mixing method is high-energy ball milling, the speed of the high-energy ball milling is 700 rpm, the time of the high-energy ball milling is 20 minutes, to obtain a first mixture;

[0046] S3, adding a low eutectic solvent to the first mixture for mixing, wherein the molar ratio of the gallium-containing metal source to the low eutectic solvent is 1:0.1, the low eutectic solvent is a mixture of choline chloride and oxalic acid, the molar ratio of choline chloride to oxalic acid is 1:3, the mixing method is high-energy ball milling, the rotation speed of the high-energy ball milling is 900 rpm, and the time of the high-energy ball milling is 50 min, to obtain a second mixture;

[0047] S4, transferring the second mixture to a reactor, wherein the temperature in the reactor is 175°C, the temperature is programmed, the heating rate is 12°C / min, the reaction is fully carried out under an argon atmosphere, the gas flow rate is 40cc / min, and the reaction time is 10h;

[0048] S5. The obtained reaction product is cooled and then ground to obtain high-purity gallium oxalate.

[0049] In this embodiment, the conversion rate of gallium oxalate is 99.8%, and the purity of gallium oxalate is 99.98%.

[0050] Example 4

[0051] A solid phase synthesis method for high-purity gallium oxalate comprises the following steps:

[0052] S1, grinding gallium-containing metal source gallium oxyhydroxide and oxalic acid respectively, wherein the molar ratio of the gallium-containing metal source to oxalic acid is 1:1, to obtain gallium-containing metal source powder and oxalic acid powder, wherein the particle size of the gallium-containing metal source powder and oxalic acid powder is less than 1 μm;

[0053] S2, mixing the gallium-containing metal source powder and the oxalic acid powder ground in step S1, the mixing method is high-energy ball milling, the speed of the high-energy ball milling is 800 rpm, and the time of the high-energy ball milling is 30 minutes, to obtain a first mixture;

[0054] S3, adding a low eutectic solvent to the first mixture for mixing, wherein the molar ratio of the gallium-containing metal source to the low eutectic solvent is 1:0.2, the low eutectic solvent is a mixture of choline chloride and oxalic acid, the molar ratio of choline chloride to oxalic acid is 1:4, the mixing method is high-energy ball milling, the rotation speed of the high-energy ball milling is 1000 rpm, and the time of the high-energy ball milling is 60 min, to obtain a second mixture;

[0055] S4, transferring the second mixture to a reactor, wherein the temperature in the reactor is 180°C, the temperature is programmed, the heating rate is 15°C / min, the mixture is fully reacted under a helium atmosphere, the gas flow rate is 50cc / min, and the reaction time is 20h;

[0056] S5. The obtained reaction product is cooled and then ground to obtain high-purity gallium oxalate.

[0057] In this embodiment, the conversion rate of gallium oxalate is 99.8%, and the purity of gallium oxalate is 99.99%.

[0058] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A solid phase synthesis method of high-purity gallium oxalate, characterized in that: The following steps are involved: S1, grinding the gallium-containing metal source and oxalic acid respectively to obtain gallium-containing metal source powder and oxalic acid powder; S2, mixing the gallium-containing metal source powder and the oxalic acid powder ground in step S1 to obtain a first mixture; S3, adding a deep eutectic solvent to the first mixture and mixing to obtain a second mixture; S4, transferring the second mixture to a reactor, raising the temperature by a program, and reacting the mixture fully under an inert atmosphere; S5. The obtained reaction product is cooled and then ground to obtain high-purity gallium oxalate.

2. The solid phase synthesis method of high-purity gallium oxalate according to claim 1, characterized in that: The gallium-containing metal source includes any one of gallium hydroxide and gallium oxyhydroxide.

3. The solid phase synthesis method of high-purity gallium oxalate according to claim 1, characterized in that: The particle sizes of the gallium-containing metal source powder and the oxalic acid powder are less than 1 μm.

4. The solid phase synthesis method of high-purity gallium oxalate according to claim 1, characterized in that: The low eutectic solvent is a mixture of choline chloride and oxalic acid, and the molar ratio of choline chloride to oxalic acid is 1:1-4.

5. The solid phase synthesis method of high-purity gallium oxalate according to claim 1, characterized in that: The molar ratio of the gallium-containing metal source to oxalic acid is 1:1, and the molar ratio of the gallium-containing metal source to the low eutectic solvent is 1:0.02-0.

2.

6. The solid phase synthesis method of high-purity gallium oxalate according to claim 1, characterized in that: The mixing method is high energy ball milling.

7. The solid phase synthesis method of high-purity gallium oxalate according to claim 6, characterized in that: In step S2, the rotation speed of the high-energy ball mill is 600-800 rpm, and the time of the high-energy ball mill is 10-30 min; In step S3, the rotation speed of the high energy ball mill is 800-1000 rpm, and the time of the high energy ball mill is 30-60 min.

8. The solid phase synthesis method of high-purity gallium oxalate according to claim 1, characterized in that: The temperature in the reactor is 160-180° C., the heating rate is 5-15° C. / min, and the reaction time is 2-20 h.

9. The solid phase synthesis method of high-purity gallium oxalate according to claim 1, characterized in that: The inert atmosphere is any one of nitrogen, argon and helium, and the gas flow rate is 10 to 50 cc / min.