Dialkyl dithiophosphate compound, preparation method thereof and application of dialkyl dithiophosphate compound as lubricating grease additive

By preparing dialkyl dithiophosphate compounds as additives for composite lithium-based greases at high temperatures, the problems of insufficient friction reduction, anti-wear and extreme pressure performance at high temperatures are solved, and excellent friction reduction is achieved It also improves extreme pressure performance while avoiding corrosion and odor problems. It is suitable for high-end grease applications.

CN119060089AActive Publication Date: 2024-12-03QINGDAO RESOURCE CHEM & NEW MATERIALS RES CENT +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411250558.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-03
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The existing anti-wear and extreme pressure additives have insufficient friction reduction, anti-wear and extreme pressure properties at high temperatures, and are prone to corrosion and large odors, which limits their application in high-end greases.

Method used

Develop a high-temperature extreme pressure anti-wear additive dialkyl dithiophosphate compound, which is prepared by reacting diphosphorus pentasulfide with alkylphenol at room temperature, and then mixing it with methacrylic acid and amine catalysts, and distillation under reduced pressure Extreme pressure anti-wear additive, used in composite lithium-based greases.

Benefits of technology

It significantly improves the friction reduction, wear and extreme pressure performance of greases, and is free of halogen and metals, environmentally friendly and economical, and is suitable for extreme pressure additives for high-performance greases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a dialkyl dithiophosphate compound, a preparation method thereof and application of the dialkyl dithiophosphate compound as a lubricating grease additive. The preparation method comprises the following steps: mixing methacrylic acid, an amine catalyst and dialkyl dithiophosphoric acid, stirring at room temperature for 1-3 hours, heating to 60-80 DEG C, stirring for 3-6 hours, and after the reaction is finished, removing a solvent and methacrylic acid which is not completely reacted in a reduced pressure distillation manner, so as to obtain the dialkyl dithiophosphate compound. Starting with the polarity of compound molecules, the compound which is novel in structure, good in wear resistance and extreme pressure performance and free of halogen, metal and other elements is designed and prepared, and the compound is environmentally friendly and economical and is expected to be widely applied to the fields of lubrication engineering and industry as a lubricating grease additive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lubricating additives and relates to a dialkyl dithiophosphate compound and a preparation method thereof and application thereof as a grease additive. Background Art

[0002] Reducing friction and wear of the main friction pairs of mechanical equipment, reducing energy consumption and reducing environmental pollution are the three major issues facing the design, manufacture and use of modern machinery, and grease plays a key role. Grease has the advantages of strong pressure resistance, good buffering performance, not easy to lose, good sealing and viscosity-temperature performance, etc., making it an indispensable lubricant. As an important component of lubricants, the role of its additives cannot be ignored. Anti-wear and extreme pressure additives have become a very important type of additives in the field of lubrication because they have the functions of improving the tribological properties of lubricating grease, increasing load-bearing capacity, reducing friction resistance, and reducing wear and abrasion.

[0003] Some commonly used compound anti-wear and extreme pressure additives, such as chlorine-containing extreme pressure anti-wear agents, sulfur-containing extreme pressure anti-wear agents, metal salt extreme pressure anti-wear agents, etc., are easy to act on metal surfaces because of the polar groups contained in their molecular structures. Due to the effect of friction heat, these groups are easy to react chemically on the surfaces of the friction pairs in contact with each other, thereby forming a friction film with extreme pressure and anti-wear effects on the friction surface. However, these additives are prone to corrosion, have strong odors, and produce ash, etc., and their application in high-end energy greases is limited. Therefore, it is of great significance to develop new high-performance extreme pressure anti-wear additives.

[0004] Therefore, this patent starts from the molecular structure design of anti-wear and extreme pressure additives, prepares high-temperature extreme pressure anti-wear additives, and explores their friction reduction and anti-wear properties and extreme pressure properties in composite lithium-based grease. Summary of the invention

[0005] The present invention aims to provide a high-temperature extreme pressure anti-wear agent dialkyl dithiophosphate compound and a preparation method thereof, which is used as an additive for lubricating grease. The present invention combines the harsh service conditions of lubricating grease to develop and design a new type of additive with excellent extreme pressure and anti-wear performance at high temperature. This type of additive can significantly improve the key performances such as friction reduction, anti-wear, and extreme pressure in composite lithium-based lubricating grease, solving the technical problem of insufficient friction reduction, anti-wear, and extreme pressure performance of lubricating grease at high temperature.

[0006] The high-temperature extreme pressure anti-wear agent dialkyl dithiophosphate compound of the present invention and the preparation method thereof comprise the following steps: (1) Add phosphorus pentasulfide to toluene solvent at room temperature, then add alkylphenol, and stir the reaction at 60°C-80°C for 10-16 hours. After the reaction is completed, remove the unreacted phosphorus pentasulfide by hot filtration, and remove the solvent and unreacted alkylphenol by reduced pressure distillation at 90°C-110°C to obtain dialkyl dithiophosphoric acid.

[0007] The alkylphenol is n-nonylphenol, n-dodecylphenol or n-pentadecylphenol; and the mass ratio of phosphorus pentasulfide to the alkylphenol is 1:2-1:3.

[0008] (2) Methacrylic acid, an amine catalyst and dialkyl dithiophosphoric acid are mixed, stirred at room temperature for 1-3 hours, then heated to 60°C-80°C and stirred for 3-6 hours. After the reaction is completed, the solvent and unreacted methacrylic acid are removed by reduced pressure distillation at 90°C-130°C to obtain dialkyl dithiophosphoric acid compounds, which are high-temperature extreme pressure and anti-wear additives.

[0009] The amine catalyst is triethylamine, tert-butyl primary amine or diisooctylamine; the mass ratio of methacrylic acid to dialkyl dithiophosphorus is 1:1-1:2; and the mass ratio of methacrylic acid to the amine catalyst is 24:1-26:1.

[0010] The structural formula of dialkyl dithiophosphate compounds is: ; Wherein, R is n-nonyl, n-dodecyl or n-pentadecyl.

[0011] The dialkyl dithiophosphate compounds in the present invention are used as additives for composite lithium-based greases, which can significantly reduce the friction coefficient and wear spot diameter of the base grease, exhibiting excellent friction reduction and anti-wear properties, and can significantly increase the maximum non-seizure load and sintering load of the base grease, exhibiting excellent extreme pressure properties, and can be used as extreme pressure additives for high-performance greases.

[0012] Beneficial effects of the present invention: 1. High-temperature extreme-pressure anti-wear additives Dialkyl dithiophosphate compounds have a novel structure and, as an additive in composite lithium-based greases, have excellent friction reduction, anti-wear and extreme pressure properties, solving the technical problem of insufficient friction reduction, anti-wear and extreme pressure properties of greases at high temperatures.

[0013] 2. The present invention starts from the polarity of compound molecules and designs and prepares a compound with novel structure, good anti-wear and extreme pressure properties, and does not contain halogen, metal and other elements. It is environmentally friendly and economical, and is expected to be widely used as a grease additive in lubrication engineering and industrial fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is the TPTP NMR result of dialkyl dithiophosphate compounds; Figure 2 This is the NMR result of dialkyl dithiophosphate compound DPTP; Figure 3 These are the HPTP NMR results of dialkyl dithiophosphate compounds. DETAILED DESCRIPTION

[0015] The present invention is further explained below with reference to specific embodiments.

[0016] Example 1 At room temperature, add 5 g of phosphorus pentasulfide to a flask containing 50 ml of toluene solvent, connect the exhaust gas treatment device, add 16.52 g of n-nonylphenol to the flask, and then stir and react at 60°C for 14 h. After the reaction is completed, the unreacted phosphorus pentasulfide is removed by hot filtration, and the solvent and unreacted nonylphenol are removed by vacuum distillation at 110°C to obtain dinonylphenol dithiophosphoric acid. Add 6.52 g of methacrylic acid, 0.26 g of triethylamine and 14.01 g of dibutylphenol dithiophosphoric acid to a flask equipped with a condenser, stir at room temperature for 2.5 h, then heat to 75°C and continue stirring for 5 h. After the reaction is completed, the solvent and unreacted methacrylic acid are removed by vacuum distillation at 110°C to obtain di-n-nonylphenol dithiophosphoric acid ester, recorded as TPTP. The prepared compound was subjected to nuclear magnetic resonance analysis, and the results are as follows Figure 1 As shown. Figure 1 It can be seen that [DPTP] 1 H NMR (chloroform-d, 600 MHz) δ0.47-1.78 (m, 41H, -CH3-CH2), 2.62-3.39 (m, 3H, -CH2-CH), 6.82-7.34 (m, 8H, CH).

[0017] 10.88g 12-hydroxystearic acid and 0.85g azelaic acid were dissolved in 70.40g base oil PAO40 at 80°C, and then 1.92g saturated lithium hydroxide aqueous solution was added thereto. The saponification reaction was carried out at 80°C for 1.5 hours. The mixed system was further heated to 220°C and refined at high temperature for 5 minutes. Then 17.60g 5750 lubricating oil (NYCOBASE 5750 lubricating oil of French NYCO (Chinese name Nico)) was added, and the mixture was naturally cooled to room temperature. The mixture was ground three times using a three-roll grinder to obtain a composite lithium-based grease, recorded as LCG.

[0018] 1 g of TPTP was added to 99 g of LCG, and after being fully stirred, the mixture was ground three times using a three-roll mill to obtain a grease composition containing 1% TPTP by mass, which was recorded as LCG+1% TPTP.

[0019] Example 2 The preparation process of TPTP is the same as that of Example 1.

[0020] The preparation process of LCG is the same as that of Example 1.

[0021] 2 g of TPTP was added to 98 g of LCG, and after being fully stirred, the mixture was ground three times using a three-roll mill to obtain a grease composition containing 2% TPTP by mass, which was recorded as LCG+2% TPTP.

[0022] Example 3 The preparation process of TPTP is the same as that of Example 1.

[0023] The preparation process of LCG is the same as that of Example 1.

[0024] 3 g of TPTP was added to 97 g of LCG, and after being fully stirred, the mixture was ground three times using a three-roll mill to obtain a grease composition containing 3% TPTP by mass, which was recorded as LCG+3% TPTP.

[0025] Example 4 At room temperature, 5 g of phosphorus pentasulfide was added to a flask containing 50 ml of toluene solvent, and the tail gas treatment device was connected. 19.68 g of n-dodecylphenol was added to the flask, and then stirred at 80°C for 16 h. After the reaction was completed, the unreacted phosphorus pentasulfide was removed by hot filtration, and the solvent and the unreacted n-dodecylphenol were removed by vacuum distillation at 110°C to obtain di-n-dodecylphenol dithiophosphoric acid. 2.13 g of methyl acrylic acid, 0.18 g of tert-butyl primary amine and 16.98 g of di-n-dodecylphenol dithiophosphoric acid were added to a flask equipped with a condenser, stirred at room temperature for 3 h, then heated to 80°C and continued to stir for 6 h. After the reaction was completed, the solvent and the unreacted methacrylic acid were removed by vacuum distillation at 120°C to obtain di-n-dodecylphenol dithiophosphoric acid ester, recorded as DPTP. The prepared compound was subjected to nuclear magnetic resonance analysis, and the results were as follows Figure 2 As shown. Figure 2 It can be seen that [DPTP] 1 H NMR(chloroform-d, 600 MHz) δ 0.30-0.92(m,12H,-CH3),2.79-3.45(m,3H,-CH2,-CH),6.94-7.35(m,8H,-CH).

[0026] The preparation process of LCG is the same as that of Example 1.

[0027] 1 g of DPTP was added to 99 g of LCG, and after being fully stirred, it was ground three times using a three-roll mill to obtain a grease composition containing 1% DPTP by mass, which was recorded as LCG+1% DPTP.

[0028] Example 5 The preparation process of DPTP is the same as that of Example 4.

[0029] The preparation process of LCG is the same as that of Example 1.

[0030] 2 g of DPTP was added to 98 g of LCG, and after being fully stirred, it was ground three times using a three-roll mill to obtain a grease composition containing 2% DPTP by mass, which was recorded as LCG+2% DPTP.

[0031] Example 6 The preparation process of DPTP is the same as that of Example 4.

[0032] The preparation process of LCG is the same as that of Example 1.

[0033] 3 g of DPTP was added to 97 g of LCG, and after being fully stirred, it was ground three times using a three-roll mill to obtain a grease composition containing 3% DPTP by mass, which was recorded as LCG+3% DPTP.

[0034] Example 7 At room temperature, add 5 g of phosphorus pentasulfide to a flask containing 50 ml of toluene solvent, connect the tail gas treatment device, add 23.88 g of n-pentadecylphenol to the flask, and then stir and react at 80°C for 16 h. After the reaction is completed, the unreacted phosphorus pentasulfide is removed by hot filtration, and the solvent and the unreacted n-pentadecylphenol are removed by vacuum distillation at 110°C to obtain dipentadecylphenol dithiophosphoric acid. Add 2.13 g of methacrylic acid, 0.60 g of diisooctylamine and 19.18 g of dipentadecylphenol dithiophosphoric acid to a flask equipped with a condenser, stir at room temperature for 3 h, then heat to 80°C and continue stirring for 6 h. After the reaction is completed, remove the solvent and the unreacted methacrylic acid by vacuum distillation at 130°C to obtain dipentadecylphenol dithiophosphoric acid ester, recorded as HPTP. The prepared compound was subjected to nuclear magnetic resonance analysis, and the results are as follows Figure 3 As shown. Figure 3 It can be seen that [HPTP] 1H NMR (chloroform-d, 600 MHz) δ 0.80(t, 6H, -CH3), 1.24 (s, 56H, -CH2), 1.57 (s, 3H, -CH3), 2.44-2.54 (m, 2H, -CH2), 3.02 (s, 1H, -CH), 6.88-7.21 (m, 8H, -CH).

[0035] The preparation process of LCG is the same as that of Example 1.

[0036] 1 g of HPTP was added to 99 g of LCG, and after being fully stirred, it was ground three times using a three-roll mill to obtain a grease composition containing 1% HPTP by mass, which was recorded as LCG+1% HPTP.

[0037] Example 8 The preparation process of HPTP is the same as that of Example 7.

[0038] The preparation process of LCG is the same as that of Example 1.

[0039] 2 g of HPTP was added to 98 g of LCG, and after being fully stirred, the mixture was ground three times using a three-roll mill to obtain a grease composition containing 2% HPTP by mass, which was recorded as LCG+2% HPTP.

[0040] Example 9 The preparation process of HPTP is shown in Example 7.

[0041] The preparation process of LCG is shown in Example 1.

[0042] 3 g of HPTP was added to 97 g of LCG, and after being fully stirred, the mixture was ground three times using a three-roll mill to obtain a grease composition containing 3% HPTP by mass, which was recorded as LCG+3% HPTP.

[0043] Comparative Example The preparation process of LCG is the same as that of Example 1. No additives are added to LCG.

[0044] Tribological performance test: Taking TPTP1 prepared in Example 1 of the present invention as an example, a four-ball friction and wear tester was used to examine its high-temperature friction reduction and anti-wear performance as a composite lithium-based grease additive, and compared it with the LCG base grease in the comparative example.

[0045] The test conditions are: load 392 N, temperature: room temperature, 75℃, 150℃, speed 1200 r / min, test time 60min, the test balls are all GCr15 bearing steel, diameter 12.7 mm, hardness HRC 60-63. The friction coefficient (f) is recorded during the test. After the friction test, the wear spot diameter (WSD) of the steel ball is detected by optical microscopy. The tribological performance test results are shown in Table 1.

[0046] From the tribological performance test results in Table 1, it can be seen that the high-temperature extreme pressure anti-wear agent in the present invention, as an additive for composite lithium-based grease, can significantly reduce the friction coefficient and wear spot diameter of the base grease at room temperature, 75°C and high temperature (150°C), showing excellent friction reduction and anti-wear performance, and can be used as a high-temperature wear reduction and anti-wear additive for high-performance grease.

[0047] Extreme pressure performance test: Taking the TPTP prepared in Example 1 of the present invention as an example, its extreme pressure performance as a composite lithium-based grease additive was examined on an extreme pressure four-ball tester, and compared with the LCG base grease in the comparative example.

[0048] The test conditions are: speed 1770 r / min, test time 10 s, room temperature, load gradually increased, the test balls are all GCr15 bearing steel, and their physical parameters are: diameter 12.7 mm, hardness HRC 60-63. The maximum no-seizure load (P B ) and sintering load (P D ). The extreme pressure performance test results are shown in Table 2.

[0049] It can be seen from the extreme pressure performance test results in Table 2 that the high temperature extreme pressure anti-wear agent in the present invention, as an additive for composite lithium-based grease, can significantly improve the maximum non-seizure load and sintering load of the base grease, exhibiting excellent extreme pressure performance, and can be used as an extreme pressure additive for high-performance grease.

[0050] The above descriptions are only two embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A dialkyl dithiophosphate compound having the structural formula: in, R is n-nonyl, n-dodecyl or n-pentadecyl.

2. The method for preparing a dialkyl dithiophosphate compound according to claim 1, comprising the following steps: (1) adding phosphorus pentasulfide to a toluene solvent at room temperature, then adding an alkyl phenol, and stirring the mixture at 60°C-80°C for 10-16 hours. After the reaction is completed, removing the unreacted phosphorus pentasulfide by hot filtration, and removing the solvent and the unreacted alkyl phenol by vacuum distillation to obtain a dialkyl dithiophosphoric acid; (2) Mix methacrylic acid, an amine catalyst and dialkyl dithiophosphoric acid, stir at room temperature for 1-3 hours, then heat to 60°C-80°C and stir for 3-6 hours. After the reaction is completed, remove the solvent and unreacted methacrylic acid by vacuum distillation to obtain dialkyl dithiophosphoric acid ester compounds.

3. The method for preparing a dialkyl dithiophosphate compound as claimed in claim 2, characterized in that: In step (1), the alkylphenol is n-nonylphenol, n-dodecylphenol or n-pentadecylphenol.

4. The method for preparing a dialkyl dithiophosphate compound as claimed in claim 2, characterized in that: In step (1), the mass ratio of phosphorus pentasulfide to alkylphenol is 1:2-1:

3.

5. The method for preparing a dialkyl dithiophosphate compound as claimed in claim 2, characterized in that: In step (2), the amine catalyst is triethylamine, tert-butylamine or diisooctylamine.

6. The method for preparing a dialkyl dithiophosphate compound as claimed in claim 2, characterized in that: In step (2), the mass ratio of methacrylic acid to dialkyl dithiophosphorus is 1:1-1:2; the mass ratio of methacrylic acid to amine catalyst is 24:1-26:

1.

7. Use of the dialkyl dithiophosphate compound as claimed in claim 1 as an additive for lubricating grease.

8. The use of the dialkyl dithiophosphate compound as claimed in claim 7 as a grease additive, characterized in that: The grease is a composite lithium-based grease, and the preparation method of the composite lithium-based grease is as follows: 12-hydroxystearic acid and azelaic acid are dissolved in a base oil of 4 / 5 of the total mass of the base oil at 60-80°C, and then a saturated lithium hydroxide aqueous solution is added thereto, a saponification reaction is carried out at 60-80°C for 1-3 hours, the mixed system is further heated to 200-220°C for high-temperature refining for 5-10 minutes, and then a base oil of 1 / 5 of the total mass of the base oil is added, the mixture is naturally cooled to room temperature, and the mixture is ground using a three-roll grinder to obtain a composite lithium-based grease; the mass ratio of 12-hydroxystearic acid to azelaic acid is 10:1~15:1; the mass ratio of azelaic acid to the saturated lithium hydroxide aqueous solution is 1:2~1:3.

Citation Information

Patent Citations

  • Organic molybdenum ionic liquid lubricating grease extreme pressure anti-wear additive, preparation method and application

    CN117946026A

  • Boric acid ester containing sulphur and phosphorus and its preparing process and use

    CN1566293A

  • 0,0-diiso-propyl-s-(2-carboethoxyethyl)-phosphorodithioate and lubricating oil compositions containing it

    GB1569730A

  • Improvements in or relating to metal salts of phosphorodithioates

    GB991158A

  • Dithiophosphoric acid derivatives as lubricant additives

    US5362419A