Carboxylated acrylate-styrene copolymer microsphere as well as preparation method, system and application thereof
A continuous tubular reactor process for preparing carboxylated acrylate-styrene copolymer microspheres addresses the limitations of traditional methods by ensuring uniform particle size and quality, suitable for applications such as redispersible rubber powder.
Patent Information
- Application Number
- CN202310627235.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-30
AI Technical Summary
Existing methods for preparing carboxylated polymer microspheres are lengthy, complex, and difficult to scale up, with poor heat and mass transfer in batch reactions, leading to non-uniform product quality and particle size.
A continuous method using a tubular reactor to polymerize styrene and acrylate with a carboxyl functional monomer in water-based media without stabilizers or surfactants, ensuring even mixing and controlled particle formation.
The method produces carboxylated acrylate-styrene copolymer microspheres with narrow particle size distribution and clean surfaces, suitable for applications like redispersible rubber powder.
Smart Images

Figure CN119060239A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer synthesis, and in particular to carboxylated acrylate-styrene copolymer microspheres and a preparation method, system and application thereof. Background Art
[0002] Functional polymer microspheres containing carboxyl groups on the surface can be used to prepare functional materials with different structures and properties, and such materials have many applications in the fields of adsorption, catalysis and biomedicine. Usually, polymer microspheres containing carboxyl groups are prepared by copolymerizing monomers with monomers containing carboxyl groups, such as acrylic acid, methacrylic acid or maleic anhydride. Common polymerization methods include suspension polymerization, emulsion polymerization, dispersion polymerization and precipitation polymerization. The preparation process is usually to add stirring in a kettle reactor to prepare polymer microspheres containing carboxyl groups. For example, Yan Gongqin, Guan Jianguo, Gan Zhiping, Preparation and Characterization of Monodisperse P (St-co-AA) Microspheres, Polymer Materials Science and Engineering, 2007, 23 (1): 222-225. Functional microspheres can also be prepared by surface grafting polymerization, using acrylic acid as a modifier, and using a soap-free emulsion polymerization method to polymerize and graft it to polystyrene, thereby obtaining functional microspheres containing carboxyl groups on the surface. For example, Song Kaijie and Wan Hongjing, Preparation of polystyrene microspheres modified by carboxylation on the particle surface and shear thickening properties of their polyethylene glycol suspension, Polymer Materials Science and Engineering, 2018, 34(05): 170-176.
[0003] Emulsion polymerization can also be used to prepare carboxylated polymer microspheres, such as the use of emulsion polymerization combined with microwave-assisted method to prepare styrene-methacrylic acid microspheres with uniform particle size in one step. For example, Zhou Tianyu et al., Microwave-assisted preparation of styrene-methacrylic acid microspheres for separation and enrichment of triazine herbicides in rice, Journal of Jilin Normal University (Natural Science Edition), 2021, 42(03): 87-94. This process requires a surfactant, and the pre-mixed reaction solution needs to be transferred to a high-pressure microwave tank for polymer preparation. The traditional emulsion polymerization method was used to prepare polymer microspheres containing carboxyl groups on the surface. The process requires controlling the amount and method of adding emulsifiers and functional monomers, and requires a multi-step process. Zhao Ruijian, Preparation of Nano-scale Carboxyl Polymer Microspheres by Emulsion Polymerization, New Chemical Materials, 2010, 38(01): 95-98. Surface carboxyl polymer microspheres can be prepared by dispersion polymerization and soap-free emulsion polymerization combined with subsequent chemical reactions. For example, monodisperse functionalized polymethyl methacrylate microspheres with different carboxyl contents can be prepared by dispersion polymerization and soap-free emulsion polymerization, followed by saponification and hydrolysis. Chen Biyun et al., Preparation and characterization of carboxyl functionalized polymethyl methacrylate microspheres, New Chemical Materials, 2013, 41(08): 92-94. This process can control the carboxyl content on the surface of the microspheres. It requires two-step process operation and the process takes a long time. Dispersion polymerization combined with seed modification method further synthesizes carboxyl polystyrene microspheres. Qin Xue, Monodisperse preparation and characterization of carboxyl polystyrene microspheres, Guangdong Chemical Industry, 2011, 38(11): 12-13. It is a two-step process and requires the use of an electrodispersant. Precipitation polymerization can also be used to prepare carboxyl functionalized microspheres. For example, a two-step precipitation polymerization method is used to graft a shell with a low crosslinking degree of carboxyl functional groups on the surface of the core to obtain monodisperse or narrowly dispersed micrometer-sized core-shell microspheres. Jiang Xuhong, Preparation of core-shell microspheres with carboxyl groups on the surface by two-step precipitation polymerization, Polymer Materials Science and Engineering, 2012, 28(07): 132-135. This method requires the use of acetonitrile organic solvent and a two-step preparation process.
[0004] The traditional process preparation method is a batch reaction with a relatively long reaction cycle, and some process operations are relatively complicated. The batch reaction is not conducive to heat and mass transfer, and the process scale-up of the preparation process is usually difficult, and the product quality is usually difficult to control. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of the prior art that the reaction cycle of intermittent reaction is long, the process operation process is relatively complicated, the kettle reaction is not conducive to the heat transfer and mass transfer of the reaction, the process of the preparation process is not easy to scale up, the product quality is usually not easy to control, and the product particle size is not uniform. A preparation method and system of carboxylated acrylate-styrene copolymer microspheres, carboxylated acrylate-styrene copolymer microspheres prepared by the method and the application of the carboxylated acrylate-styrene copolymer microspheres are provided. The preparation method is simple and continuous to operate, and the addition ratio of materials is convenient to adjust. No stabilizer and surfactant are added in the preparation process, and the surface of the obtained polymer microspheres is clean and the particle size distribution is narrow.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing carboxylated acrylate-styrene copolymer microspheres, characterized in that the method comprises:
[0007] S1, mixing the first mixed solution and the second mixed solution uniformly to obtain a raw material solution;
[0008] S2, mixing the raw material liquid and the initiator uniformly to obtain a reaction liquid, and subjecting the reaction liquid to a polymerization reaction in a tubular reactor to obtain carboxylated acrylate-styrene copolymer microspheres;
[0009] The first mixed solution contains styrene, acrylate and a first dispersion medium; the second mixed solution contains a carboxyl functional monomer and a second dispersion medium;
[0010] The first dispersion medium and the second dispersion medium are both water.
[0011] The second aspect of the present invention provides carboxylated acrylate-styrene copolymer microspheres prepared by the preparation method described in the first aspect of the present invention.
[0012] The third aspect of the present invention provides a use of the carboxylated acrylate-styrene copolymer microspheres described in the second aspect of the present invention as redispersible rubber powder.
[0013] The fourth aspect of the present invention provides a system for preparing the carboxylated acrylate-styrene copolymer microspheres according to the second aspect of the present invention, characterized in that the system comprises: a first raw material tank (1-1), a second raw material tank (1-2), a third raw material tank (1-3), a first mixer (2-1), a second mixer (2-2), a tubular reactor (3) and a heater (4);
[0014] The first raw material tank (1-1) contains a first mixed liquid, and the second raw material tank (1-2) contains a second mixed liquid;
[0015] The first raw material tank (1-1) and the second raw material tank (1-2) are respectively connected to the inlet of the first mixer (2-1) and are used to send the first mixed liquid and the second mixed liquid into the first mixer (2-1) to obtain raw material liquids;
[0016] The third raw material tank (1-3) contains an initiator;
[0017] The third raw material tank (1-3) is connected to the inlet of the second mixer (2-2) and is used to feed the initiator into the first mixer (2-1);
[0018] The outlet of the first mixer (2-1) is connected to the inlet of the second mixer (2-2), so as to feed the raw material liquid into the second mixer (2-2) and mix it with the initiator to obtain a reaction liquid;
[0019] The inlet of the tubular reactor (3) is connected to the outlet of the second mixer (2-2), and a heater (4) is provided outside the tubular reactor (3) for polymerizing the reaction solution to obtain the carboxylated acrylate-styrene copolymer microspheres.
[0020] Through the above technical scheme, the carboxylated acrylate-styrene copolymer microspheres and the preparation method, system and application thereof provided by the present invention achieve the following beneficial effects: the method is easy to operate, the process is continuous, the addition ratio of materials is convenient to adjust, and no stabilizer or surfactant is added during the preparation process. The surface of the obtained polymer microspheres is clean and the particle size distribution is narrow. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a scanning electron microscope image of the carboxylated acrylate-styrene copolymer microspheres prepared in Example 1 of the present invention;
[0022] Figure 2 Schematic diagram of a system for preparing carboxylated acrylate-styrene copolymer microspheres according to Example 1 of the present invention.
[0023] Description of Reference Numerals
[0024] 1-1 the first raw material tank; 1-2 the second raw material tank; 1-3 the third raw material tank; 2-1 the first mixer; 2-2 the second mixer; 3 the tubular reactor; 4 the heater; 5-1 the first chromatography pump; 5-2 the second chromatography pump; 5-3 the third chromatography pump; 6-1 the first one-way valve; 6-2 the second one-way valve; 6-3 the third one-way valve; 6-4 the fourth one-way valve; 6-5 the fifth one-way valve; 7 the collecting tank. DETAILED DESCRIPTION
[0025] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0026] The first aspect of the present invention provides a method for preparing carboxylated acrylate-styrene copolymer microspheres, characterized in that the method comprises:
[0027] S1, mixing the first mixed solution and the second mixed solution uniformly to obtain a raw material solution;
[0028] S2, mixing the raw material liquid and the initiator uniformly to obtain a reaction liquid, and subjecting the reaction liquid to a polymerization reaction in a tubular reactor to obtain carboxylated acrylate-styrene copolymer microspheres;
[0029] The first mixed solution contains styrene, acrylate and a first dispersion medium; the second mixed solution contains a carboxyl functional monomer and a second dispersion medium;
[0030] The first dispersion medium and the second dispersion medium are both water.
[0031] In the present invention, the dispersion medium is water, which is immiscible with the reaction monomer raw materials, can reduce the viscosity of the reaction raw materials, and provide a reaction site, remove the reaction heat, and make the formed polymer form a colloidal dispersion system. Furthermore, after mixing styrene and acrylate, and then mixing with carboxyl functional monomers, the reaction raw materials can be mixed more evenly, and the proportion of structural units in the synthetic polymer can be conveniently adjusted.
[0032] According to the present invention, in the first mixed solution, the mass concentration of styrene is 5-25%, preferably 5-22.5%.
[0033] According to the present invention, in the first mixed solution, the mass concentration of the acrylic ester is 5-15%, preferably 6-14%.
[0034] According to the present invention, the acrylate has a structure shown in formula (1):
[0035]
[0036] Among them, R1 is H or a C1-C6 alkyl group, and R2 is a C1-C6 alkyl group.
[0037] Preferably, R1 is H or methyl, and R2 is C1-C3 alkyl.
[0038] According to the present invention, the carboxyl functional monomer has a structure shown in formula (2):
[0039]
[0040] Wherein, R3 is H or a C1-C6 alkyl group.
[0041] According to a particularly preferred embodiment of the present invention, the carboxyl functional monomer is selected from methacrylic acid and acrylic acid.
[0042] In the present invention, the carboxyl functional monomer is selected from methacrylic acid and acrylic acid, which can make the prepared copolymer microspheres have good uniformity and a narrower particle size dispersion coefficient.
[0043] According to the present invention, the carboxyl functional monomer is selected from methacrylic acid and acrylic acid, wherein the methacrylic acid in the second mixed solution accounts for 70%-95% of the total mass of the carboxyl functional monomer.
[0044] Furthermore, in the second mixed solution, methacrylic acid accounts for 70-90% of the total mass of the carboxyl functional monomers.
[0045] According to the present invention, the mass concentration of the carboxyl functional monomer in the second mixed liquid is 10-40%, preferably 11-30%.
[0046] According to the present invention, the initiator is an aqueous solution of persulfate, preferably an aqueous solution of ammonium persulfate and / or an aqueous solution of potassium persulfate.
[0047] According to the present invention, in the persulfate aqueous solution, the mass concentration of the persulfate is 1-20%.
[0048] In the present invention, the mass concentration of the persulfate satisfies the above range and can provide a suitable reaction rate.
[0049] Furthermore, in the persulfate aqueous solution, the mass concentration of the persulfate is 1-15%.
[0050] According to the present invention, the inner diameter of the tubular reactor is 0.1-2 mm.
[0051] In the present invention, the inner diameter of the tubular reactor satisfies the above range, which can easily remove the reaction heat during the reaction and improve the uniformity of the polymer microspheres.
[0052] Furthermore, the inner diameter of the tubular reactor is 0.1-1.5 mm.
[0053] According to the present invention, the length of the tubular reactor is 200-10000 mm.
[0054] In the present invention, the length of the tubular reactor satisfies the above range, which can ensure the smooth progress of the reaction and ensure a suitable conversion rate.
[0055] Furthermore, the length of the tubular reactor is 500-10000 mm.
[0056] According to the present invention, in step S1, the first mixed liquid and the second mixed liquid are mixed in a first mixer to obtain a raw material liquid.
[0057] In the present invention, the first mixer is a T-type mixer, which can fully and evenly mix the reaction raw materials, and further improve the particle size dispersion coefficient of the prepared polymer microspheres.
[0058] According to the present invention, the delivery rate of the first mixed liquid is 1-15 ml / min.
[0059] According to the present invention, the delivery rate of the second mixed liquid is 0.1-3 ml / min.
[0060] According to the present invention, the delivery rate of the first mixed liquid and the delivery rate of the second mixed liquid respectively meet the above ranges, which can better control the structure of the polymer obtained by the reaction and ensure the formation of a dispersed system.
[0061] According to the present invention, in step S2, the raw material liquid and the initiator are mixed in a second mixer to obtain a reaction liquid.
[0062] In the present invention, the second mixer is a T-type mixer, which can ensure that the reaction materials are mixed evenly.
[0063] According to the present invention, the delivery rate of the raw material liquid is 1.1-18 ml / min, preferably 1.1-15 ml / min.
[0064] According to the present invention, the delivery rate of the initiator is 1-15 ml / min, preferably 1-10 ml / min.
[0065] According to the present invention, the conditions of the polymerization reaction include: reaction temperature of 65-95° C., preferably 65-90° C.; reaction time of 2-24 h, preferably 6-18 h.
[0066] The second aspect of the present invention provides carboxylated acrylate-styrene copolymer microspheres prepared by the preparation method described in the first aspect of the present invention.
[0067] According to the present invention, in the copolymer microspheres, the molar content of the structural units provided by styrene is 30-60%.
[0068] According to the present invention, in the copolymer microspheres, the molar content of the structural units provided by acrylic acid ester is 20-55%.
[0069] According to the present invention, in the copolymer microspheres, the molar content of the structural units provided by the carboxyl functional monomers is 10-30%.
[0070] In the present invention, when the molar content of the structural unit provided by styrene, the molar content of the structural unit provided by acrylate, and the molar content of the structural unit provided by the carboxyl functional monomer in the copolymer microspheres each meet the above ranges, the prepared copolymer microspheres have uniform particle size, excellent morphology, clean microsphere surface, and can be used as redispersible rubber powder.
[0071] Further, according to the present invention, in the copolymer microspheres, the molar content of the structural units provided by styrene is 35-54%.
[0072] According to the present invention, in the copolymer microspheres, the molar content of the structural units provided by acrylic acid ester is 26-45%.
[0073] According to the present invention, in the copolymer microspheres, the molar content of the structural units provided by the carboxyl functional monomers is 17-23%.
[0074] In the present invention, in the copolymer microspheres, the sum of the molar content of the structural unit provided by styrene, the molar content of the structural unit provided by acrylate and the molar content of the structural unit provided by the carboxyl functional monomer is 100%.
[0075] According to a particularly preferred embodiment of the present invention, the carboxyl functional monomer is selected from methacrylic acid and acrylic acid. In the copolymer microspheres, the molar content of the structural unit provided by methacrylic acid is 1-20%, the molar content of the structural unit provided by acrylic acid is 1-20%, and the total content of the structural unit provided by the carboxyl functional monomer is 10-30%.
[0076] According to the present invention, the average particle size of the copolymer microspheres is 200-1200 nm, preferably 200-900 nm.
[0077] According to the present invention, the weight average particle size of the copolymer microspheres is 200-1400 nm, preferably 200-1200 nm.
[0078] According to the present invention, the particle size dispersion coefficient of the copolymer microspheres is 1.002-1.02, preferably 1.005-1.02.
[0079] The third aspect of the present invention provides a use of the carboxylated acrylate-styrene copolymer microspheres described in the second aspect of the present invention as redispersible rubber powder.
[0080] In the present invention, when the carboxylated acrylate-styrene copolymer microspheres are used as redispersible rubber powder, the residual amount thereof is not higher than 0.23 wt %, preferably not higher than 0.17 wt %.
[0081] The fourth aspect of the present invention provides a system for preparing the carboxylated acrylate-styrene copolymer microspheres according to the second aspect of the present invention, characterized in that the system comprises: a first raw material tank (1-1), a second raw material tank (1-2), a third raw material tank (1-3), a first mixer (2-1), a second mixer (2-2), a tubular reactor (3) and a heater (4);
[0082] The first raw material tank (1-1) contains a first mixed liquid, and the second raw material tank (1-2) contains a second mixed liquid;
[0083] The first raw material tank (1-1) and the second raw material tank (1-2) are respectively connected to the inlet of the first mixer (2-1) and are used to send the first mixed liquid and the second mixed liquid into the first mixer (2-1) to obtain raw material liquids;
[0084] The third raw material tank (1-3) contains an initiator;
[0085] The third raw material tank (1-3) is connected to the inlet of the second mixer (2-2) and is used to feed the initiator into the first mixer (2-2);
[0086] The outlet of the first mixer (2-1) is connected to the inlet of the second mixer (2-2), so as to feed the raw material liquid into the second mixer (2-2) and mix it with the initiator to obtain a reaction liquid;
[0087] The inlet of the tubular reactor (3) is connected to the outlet of the second mixer (2-2), and a heater (4) is provided outside the tubular reactor (3) for polymerizing the reaction solution to obtain the carboxylated acrylate-styrene copolymer microspheres.
[0088] In the present invention, the first raw material tank (1-1) is provided with a stirring device for stirring and mixing the raw materials therein uniformly.
[0089] In the present invention, there is no particular limitation on the stirring conditions, as long as the raw materials can be mixed evenly. For example, the rotation speed may be 50-300 rpm.
[0090] In the present invention, there is no particular limitation on the type and heating method of the heater, as long as it can provide the temperature required for the polymerization reaction, for example, it can be an oil bath or a water bath with a temperature control range of 10-220°C and a temperature control accuracy of ±1°C.
[0091] According to the present invention, the system further comprises a pump (5), a one-way valve (6) and a collection tank (7);
[0092] The inlet of the collecting tank (7) is connected to the outlet of the tubular reactor (3) and is used to collect the carboxylated acrylate-styrene copolymer microspheres.
[0093] In the present invention, there is no particular requirement for the type of the pump, and it may be a chromatography pump, for example.
[0094] In the present invention, there is no special requirement for the working conditions of the pump, as long as it can meet the liquid delivery rate specified in the present invention. For example, the maximum working pressure of the pump is 2.5MPa, and the flow range of the chromatographic pump is 0.05-50 ml / min.
[0095] Combination Figure 2 , the method and system of the present invention are further described:
[0096] S1, placing styrene, methacrylate and water in a first raw material tank (1-1), and mixing the above raw materials at a rotation speed of 50-300 rpm to obtain a first mixed solution, wherein the mass concentration of styrene in the first mixed solution is 5-25%, and the mass concentration of methyl methacrylate is 5-15%;
[0097] Mixing carboxyl functional monomer and water in a second raw material tank (1-2) to obtain a second mixed solution;
[0098] The first raw material tank (1-1) is connected to the inlet of the first mixer (2-1) via the first chromatographic pump (5-1) and the first one-way valve (6-1), and the second raw material tank (1-2) is connected to the inlet of the first mixer (2-1) via the second chromatographic pump (5-2) and the second one-way valve (6-2), and is used to transport the first mixed liquid and the second mixed liquid to the first mixer (2-1) respectively to obtain raw material liquids;
[0099] S2, the third raw material tank (1-3) contains an initiator, and the third raw material tank (1-3) is connected to the inlet of the second mixer (2-2) through the third chromatographic pump (5-3) and the third one-way valve (6-3), and is used to transport the initiator to the first mixer (2-2), wherein the initiator is an aqueous solution of persulfate, and the mass concentration of the persulfate is 1-20%;
[0100] The outlet of the first mixer (2-1) is connected to the inlet of the second mixer (2-2) via a fourth one-way valve (6-4), so as to transport the raw material liquid to the second mixer (2-2) and mix it with the initiator in the first mixer (2-2) to obtain a reaction liquid;
[0101] S3, the inlet of the tubular reactor (3) and the outlet of the second mixer (2-2) are connected through a fifth one-way valve (6-5), and a heater (4) is provided outside the tubular reactor (3), and the reaction liquid is polymerized in the tubular reactor to obtain carboxylated acrylate-styrene copolymer microspheres; the conditions of the polymerization reaction include: a reaction temperature of 65-95°C and a reaction time of 2-24h;
[0102] S4. The inlet of the collecting tank (7) is connected to the outlet of the tubular reactor (3) for collecting the carboxylated acrylate-styrene copolymer microspheres.
[0103] Wherein, the inner diameter of the tubular reactor is 0.1-2 mm and the length is 200-10000 mm;
[0104] The delivery rate of the first mixed liquid is 1-15 ml / min, and the delivery rate of the second mixed liquid is 0.1-3 ml / min;
[0105] The delivery rate of the raw material liquid is 1.1-18 ml / min, and the delivery rate of the initiator is 1-15 ml / min.
[0106] The present invention will be described in detail below by way of examples. In the following examples,
[0107] The morphology of the polymers was observed using a Hitachi S-4800 scanning electron microscope.
[0108] The particle size of the polymer was measured by scanning electron microscopy graphics software;
[0109] The content of each structural unit in the polymer is tested by 1H NMR. The testing method is to calculate the content of each structural unit by the ratio of the peak area corresponding to the characteristic hydrogen in the corresponding structural unit in 1H NMR;
[0110] The number average particle size is Where n is the number of particles, di is the particle size of the i-th particle;
[0111] The weight average particle size is Where n is the number of particles, di is the particle size of the i-th particle;
[0112] The particle size distribution coefficient is P = Dw / Dn.
[0113] The raw materials involved in the examples and comparative examples are all conventional commercial products in the art.
[0114] Example 1
[0115] S1, placing styrene, methyl methacrylate and water in a first raw material tank (1-1), and mixing the above raw materials at a rotation speed of 250 rpm to obtain a first mixed solution, wherein the mass concentration of styrene in the first mixed solution is 10%, and the mass concentration of methyl methacrylate is 10%;
[0116] Methacrylic acid, acrylic acid and water are mixed evenly in a second raw material tank (1-2) to obtain a second mixed solution, wherein in the second mixed solution, methacrylic acid accounts for 85% of the total mass of the carboxyl functional monomers, acrylic acid accounts for 15% of the total mass of the carboxyl functional monomers; and the mass concentration of the carboxyl functional monomers is 20%.
[0117] The first raw material tank (1-1) is connected to the inlet of the first mixer (2-1) via the first chromatographic pump (5-1) and the first one-way valve (6-1), and the second raw material tank (1-2) is connected to the inlet of the first mixer (2-1) via the second chromatographic pump (5-2) and the second one-way valve (6-2), and is used to transport the first mixed liquid and the second mixed liquid to the first mixer (2-1) respectively to obtain raw material liquids;
[0118] S2, the third raw material tank (1-3) contains an initiator, and the third raw material tank (1-3) is connected to the inlet of the second mixer (2-2) through the third chromatographic pump (5-3) and the third one-way valve (6-3), and is used to transport the initiator to the first mixer (2-2), wherein the initiator is an aqueous solution of potassium persulfate, and the mass concentration of the potassium persulfate is 15%;
[0119] The outlet of the first mixer (2-1) is connected to the inlet of the second mixer (2-2) via a fourth one-way valve (6-4), so as to transport the raw material liquid to the second mixer (2-2) and mix it with the initiator in the first mixer (2-2) to obtain a reaction liquid;
[0120] S3, the inlet of the tubular reactor (3) and the outlet of the second mixer (2-2) are connected through a fifth one-way valve (6-5), and a heater (4) is provided outside the tubular reactor (3), and the reaction liquid is polymerized in the tubular reactor to obtain carboxylated acrylate-styrene copolymer microspheres A1; the conditions of the polymerization reaction include: a reaction temperature of 90° C. and a reaction time of 3.3 h;
[0121] S4. The inlet of the collecting tank (7) is connected to the outlet of the tubular reactor (3) to collect the carboxylated acrylate-styrene copolymer microspheres A1.
[0122] Wherein, the inner diameter of the tubular reactor is 0.5 mm and the length is 10000 mm;
[0123] The delivery rate of the first mixed liquid is 8 ml / min, and the delivery rate of the second mixed liquid is 2 ml / min;
[0124] The delivery rate of the raw material liquid is 10 ml / min, and the delivery rate of the initiator is 5 ml / min.
[0125] The morphology of polymer microsphere A1 product is as follows Figure 1 As shown. Figure 1 It can be seen that the obtained polymer microspheres A1 are monodisperse microspheres with smooth surface and uniform particle size. It has been determined that the carboxylated acrylate-styrene copolymer microspheres A1 are copolymer microspheres of styrene-methyl methacrylate-methacrylic acid-acrylic acid, and the molar content of the structural unit provided by styrene in the copolymer microspheres A1 is 39%, the molar content of the structural unit provided by methyl methacrylate is 41%, the molar content of the structural unit provided by methacrylic acid is 16%, and the molar content of the structural unit provided by acrylic acid is 4%.
[0126] The particle size of the obtained polymer microspheres A1 is 530 nm, the particle size dispersion coefficient of the polymer microspheres A1 is 1.006, the number average particle size is 530 nm, and the weight average particle size is 533 nm.
[0127] Example 2
[0128] The method of Example 1 is followed, except that:
[0129] In the first mixed solution, the mass concentration of styrene is 15%, and the mass concentration of methyl methacrylate is 12%;
[0130] In the second mixed solution, methacrylic acid accounts for 80% of the total mass of the carboxyl functional monomers, and acrylic acid accounts for 20% of the total mass of the carboxyl functional monomers; the mass concentration of the carboxyl functional monomers is 27%.
[0131] In the aqueous solution of the initiator potassium persulfate, the mass concentration of potassium persulfate is 12.5%;
[0132] The polymerization temperature was 85°C;
[0133] The inner diameter of the tubular reactor is 0.1 mm and the length is 8000 mm;
[0134] The delivery rate of the first mixed liquid is 1 ml / min, and the delivery rate of the second mixed liquid is 0.2 ml / min;
[0135] The delivery rate of the raw material liquid is 1.2 ml / min, and the delivery rate of the initiator is 1 ml / min;
[0136] The obtained polymer microspheres A2 were tested, wherein the content of each structural unit, the particle size of the copolymer microspheres A2, the particle size dispersion coefficient, the number average particle size and the weight average particle size are shown in Table 1 and Table 1 (Continued).
[0137] Example 3
[0138] The method of Example 1 is followed, except that:
[0139] In the first mixed solution, the mass concentration of styrene is 8%, and the mass concentration of methyl methacrylate is 9%;
[0140] In the second mixed solution, methacrylic acid accounts for 75% of the total mass of the carboxyl functional monomers, and acrylic acid accounts for 25% of the total mass of the carboxyl functional monomers; the mass concentration of the carboxyl functional monomers is 17%.
[0141] In the aqueous solution of the initiator potassium persulfate, the mass concentration of potassium persulfate is 17.5%;
[0142] The inner diameter of the tubular reactor is 1 mm and the length is 3000 mm;
[0143] The delivery rate of the first mixed liquid is 7 ml / min, and the delivery rate of the second mixed liquid is 2 ml / min;
[0144] The delivery rate of the raw material liquid is 9 ml / min, and the delivery rate of the initiator is 7 ml / min;
[0145] The obtained polymer microspheres A3 were tested, wherein the content of each structural unit, the particle size, particle size dispersion coefficient, number average particle size and weight average particle size of the copolymer microspheres A3 are shown in Table 1 and Table 1 (Continued).
[0146] Example 4
[0147] The method of Example 1 is followed, except that:
[0148] In the first mixed solution, the mass concentration of styrene is 5%, and the mass concentration of methyl methacrylate is 6%;
[0149] In the second mixed solution, methacrylic acid accounts for 70% of the total mass of the carboxyl functional monomers, and acrylic acid accounts for 30% of the total mass of the carboxyl functional monomers; the mass concentration of the carboxyl functional monomers is 11%.
[0150] In the aqueous solution of initiator ammonium persulfate, the mass concentration of ammonium persulfate is 20%;
[0151] The inner diameter of the tubular reactor is 1.5 mm and the length is 2000 mm;
[0152] The delivery rate of the first mixed liquid is 8.2 ml / min, and the delivery rate of the second mixed liquid is 1.8 ml / min;
[0153] The delivery rate of the raw material liquid is 10 ml / min, and the delivery rate of the initiator is 10 ml / min;
[0154] The obtained polymer microspheres A4 were tested, wherein the content of each structural unit, the particle size, particle size dispersion coefficient, number average particle size and weight average particle size of the copolymer microspheres A4 are shown in Table 1 and Table 1 (Continued).
[0155] Example 5
[0156] The method of Example 1 is followed, except that:
[0157] In the first mixed solution, the mass concentration of styrene is 20%, and the mass concentration of methyl methacrylate is 10%;
[0158] In the second mixed solution, methacrylic acid accounts for 70% of the total mass of the carboxyl functional monomers, and acrylic acid accounts for 30% of the total mass of the carboxyl functional monomers; the mass concentration of the carboxyl functional monomers is 30%.
[0159] In the aqueous solution of initiator ammonium persulfate, the mass concentration of ammonium persulfate is 5%;
[0160] The polymerization temperature is 75°C;
[0161] The inner diameter of the tubular reactor is 1.5 mm and the length is 3000 mm;
[0162] The delivery rate of the first mixed liquid is 10 ml / min, and the delivery rate of the second mixed liquid is 2.5 ml / min;
[0163] The delivery rate of the raw material liquid is 12.5 ml / min, and the delivery rate of the initiator is 10 ml / min;
[0164] The obtained polymer microspheres A5 were tested, wherein the content of each structural unit, the particle size, particle size dispersion coefficient, number average particle size and weight average particle size of the copolymer microspheres A5 are shown in Table 1 and Table 1 (Continued).
[0165] Example 6
[0166] The method of Example 1 is followed, except that:
[0167] In the first mixed solution, the mass concentration of styrene is 20%, and the mass concentration of methyl methacrylate is 15%;
[0168] In the second mixed solution, methacrylic acid accounts for 90% of the total mass of the carboxyl functional monomers, and acrylic acid accounts for 10% of the total mass of the carboxyl functional monomers; the mass concentration of the carboxyl functional monomers is 35%.
[0169] In the aqueous solution of initiator ammonium persulfate, the mass concentration of ammonium persulfate is 2%;
[0170] The polymerization temperature is 75°C;
[0171] The inner diameter of the tubular reactor is 2 mm and the length is 500 mm;
[0172] The delivery rate of the first mixed liquid is 8 ml / min; the delivery rate of the second mixed liquid is 1.5 ml / min;
[0173] The obtained polymer microspheres A6 were tested, wherein the content of each structural unit, the particle size of the copolymer microspheres A6, the particle size dispersion coefficient, the number average particle size and the weight average particle size are shown in Table 1 and Table 1 (Continued).
[0174] Example 7
[0175] The method of Example 1 is followed, except that in the first mixed solution, the mass concentration of the methacrylate is 15%.
[0176] The obtained polymer microspheres A7 were tested, wherein the content of each structural unit, the particle size, particle size dispersion coefficient, number average particle size and weight average particle size of the copolymer microspheres A7 are shown in Table 1 and Table 1 (Continued).
[0177] Example 8
[0178] The method of Example 1 is followed, except that the delivery rate of the first mixed liquid is 13 ml / min.
[0179] The obtained polymer microspheres A8 were tested, wherein the content of each structural unit, the particle size of the copolymer microspheres A8, the particle size dispersion coefficient, the number average particle size and the weight average particle size are shown in Table 1 and Table 1 (Continued).
[0180] Example 9
[0181] The method of Example 1 is followed, except that the inner diameter of the tubular reactor is 3 mm.
[0182] The obtained polymer microspheres A9 were tested, wherein the content of each structural unit, the particle size of the copolymer microspheres A9, the particle size dispersion coefficient, the number average particle size and the weight average particle size are shown in Table 1 and Table 1 (Continued).
[0183] Example 10
[0184] The method of Example 1 is followed, except that the carboxyl functional monomer is only acrylic acid.
[0185] The obtained polymer microspheres A10 were tested, wherein the content of each structural unit, the particle size, particle size dispersion coefficient, number average particle size and weight average particle size of the copolymer microspheres A10 are shown in Table 1 and Table 1 (Continued).
[0186] Comparative Example 1
[0187] According to the method of Example 1, except that no carboxyl functional monomer is contained, the first mixed solution and the initiator are directly mixed to carry out polymerization reaction, the reaction pipeline is blocked, and no polymer microspheres are obtained.
[0188] Comparative Example 2
[0189] The method of Example 1 is followed, except that the first mixed solution, the second mixed solution and the initiator are polymerized in a tank reactor to obtain copolymer microspheres D2.
[0190] The obtained polymer microspheres D2 were tested, wherein the content of each structural unit, the particle size, particle size dispersion coefficient, number average particle size and weight average particle size of the copolymer microspheres D2 are shown in Table 1 and Table 1 (Continued)
[0191] Comparative Example 3
[0192] The method of Example 1 was followed, except that the first dispersion medium and the second dispersion medium were both ethyl acetate. No polymer dispersed colloid system was obtained.
[0193] Table 1
[0194]
[0195]
[0196] It can be seen from the results in Table 1 that the polymer microspheres prepared in Examples 1 to 10 of the present invention have a narrow particle size distribution, and the particle size dispersion coefficient is no higher than 1.02. The particle size of the polymer microspheres is uniform.
[0197] Furthermore, Examples 1-6 that meet the preferred embodiments of the present invention achieve significantly better technical effects, and microspheres A1-A6 have a narrower particle size distribution, and the particle size dispersion coefficient is not higher than 1.01.
[0198] In order to further illustrate that the polymer microspheres prepared by the present invention can be used as redispersible rubber powder, 2 g of the polymer microsphere powder prepared in the embodiment and the comparative example was dispersed in 100 g of deionized water, stirred at 200 rpm for 10 minutes, filtered with a filter screen with an aperture of 38 microns, and the residual polymer that did not pass through the filter screen was dried, and the residual substance content R was tested, and the effect was tested. The results are shown in Table 2.
[0199] The calculation of the residual amount R is shown as follows:
[0200]
[0201] Wherein, w1 is the amount of residual polymer that has not passed through the filter paper, and w0 is the amount of polymer dry powder initially added.
[0202] Table 2
[0203]
[0204]
[0205] From the above description, it can be seen that the polymer microspheres prepared by this technology can be used as dispersible rubber powder, which has lower residual amount than the rubber powder obtained by traditional methods and has better redispersibility.
[0206] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing carboxylated acrylate-styrene copolymer microspheres, It is characterized in that The method comprises: S1, mixing the first mixed solution and the second mixed solution uniformly to obtain a raw material solution; S2, mixing the raw material liquid and the initiator uniformly to obtain a reaction liquid, and subjecting the reaction liquid to a polymerization reaction in a tubular reactor to obtain carboxylated acrylate-styrene copolymer microspheres; The first mixed solution contains styrene, acrylate and a first dispersion medium; the second mixed solution contains a carboxyl functional monomer and a second dispersion medium; The first dispersion medium and the second dispersion medium are both water.
2. The preparation method according to claim 1, in, In the first mixed solution, the mass concentration of styrene is 5-25%, preferably 5-22.5%; Preferably, in the first mixed solution, the mass concentration of the acrylic acid ester is 5-15%, preferably 6-14%; Preferably, the acrylate has a structure shown in formula (1): Among them, R 1 H or C 1 -C 6 The alkyl group, R 2 C 1 -C 6 The alkyl group; Preferably, R 1 is H or methyl, R 2 C 1 -C 3 The alkyl group; Preferably, the carboxyl functional monomer has a structure shown in formula (2): Among them, R 3 H or C 1 -C 6 The alkyl group; Preferably, the carboxyl functional monomer is selected from methacrylic acid and acrylic acid, wherein the methacrylic acid in the second mixed solution accounts for 70%-95% of the total mass of the carboxyl functional monomer, preferably 70-90%; Preferably, the mass concentration of the carboxyl functional monomer in the second mixed liquid is 10-40%, preferably 11-30%.
3. The preparation method according to claim 1 or 2, in, The initiator is an aqueous solution of persulfate, preferably an aqueous solution of ammonium persulfate and / or an aqueous solution of potassium persulfate; Preferably, in the persulfate aqueous solution, the mass concentration of the persulfate is 1-20%.
4. The preparation method according to any one of claims 1 to 3, in, The inner diameter of the tubular reactor is 0.1-2 mm, preferably 0.1-1.5 mm; Preferably, the length of the tubular reactor is 200-10000 mm, preferably 500-10000 mm.
5. The preparation method according to any one of claims 1 to 4, in, In step S1, the first mixed liquid and the second mixed liquid are mixed in a first mixer to obtain a raw material liquid; Preferably, the delivery rate of the first mixed solution is 1-15 ml / min, preferably 1-12.5 ml / min; Preferably, the delivery rate of the second mixed liquid is 0.1-3 ml / min, preferably 0.1-2.5 ml / min.
6. The preparation method according to any one of claims 1 to 5, in, In step S2, the raw material liquid and the initiator are mixed in a second mixer to obtain a reaction liquid; Preferably, the delivery rate of the raw material liquid is 1.1-18 ml / min, preferably 1.1-15 ml / min; Preferably, the delivery rate of the initiator is 1-15 ml / min, preferably 1-10 ml / min.
7. The preparation method according to any one of claims 1 to 6, in, The conditions of the polymerization reaction include: reaction temperature of 65-95° C., preferably 65-90° C.; reaction time of 2-24 h, preferably 3-18 h.
8. Carboxylated acrylate-styrene copolymer microspheres prepared by the preparation method according to any one of claims 1 to 7.
9. The carboxylated acrylate-styrene copolymer microspheres according to claim 8, in, In the copolymer microspheres, the molar content of the structural units provided by styrene is 30-60%, preferably 35-54%; Preferably, in the copolymer microspheres, the molar content of the structural units provided by the acrylic acid ester is 20-55%, preferably 26-45%; Preferably, in the copolymer microspheres, the molar content of the structural units provided by the carboxyl functional monomers is 10-30%, preferably 17-23%.
10. The carboxylated acrylate-styrene copolymer microspheres according to claim 8 or 9, in, The number average particle size of the copolymer microspheres is 200-1200 nm, preferably 200-900 nm; Preferably, the weight average particle size of the copolymer microspheres is 200-1400 nm, preferably 200-1200 nm; Preferably, the particle size dispersion coefficient of the copolymer microspheres is 1.002-1.02, preferably 1.005-1.
02.
11. Use of the carboxylated acrylate-styrene copolymer microspheres according to any one of claims 8 to 10 as redispersible rubber powder.
12. A system for preparing the carboxylated acrylate-styrene copolymer microspheres according to any one of claims 8 to 10, It is characterized in that The system comprises: a first raw material tank 1-1, a second raw material tank 1-2, a third raw material tank 1-3, a first mixer 2-1, a second mixer 2-2, a tubular reactor 3 and a heater 4; The first raw material tank 1-1 contains a first mixed liquid, and the second raw material tank 1-2 contains a second mixed liquid; The first raw material tank 1-1 and the second raw material tank 1-2 are respectively connected to the inlet of the first mixer 2-1, and are used to send the first mixed liquid and the second mixed liquid into the first mixer 2-1 to obtain raw material liquid; The third raw material tank 1-3 contains an initiator; The third raw material tank 1-3 is connected to the inlet of the second mixer 2-2, and is used to feed the initiator into the first mixer 2-1; The outlet of the first mixer 2-1 is connected to the inlet of the second mixer 2-2, so as to feed the raw material liquid into the second mixer 2-2 and mix it with the initiator to obtain a reaction liquid; The inlet of the tubular reactor 3 is connected to the outlet of the second mixer 2 - 2 , and a heater 4 is disposed outside the tubular reactor 3 for polymerizing the reaction solution to obtain the carboxylated acrylate-styrene copolymer microspheres.
13. The system according to claim 12, in, The system also includes a pump 5, a one-way valve 6 and a collection tank 7; The inlet of the collecting tank 7 is communicated with the outlet of the tubular reactor 3, and is used for collecting the carboxylated acrylate-styrene copolymer microspheres.
Citation Information
Patent Citations
Preparation method and application of carboxylated polystyrene microspheres
CN108264601A
Preparation method and preparation device for polyacrylamide nanoparticles
CN110054727A
Polymer nanoparticle and preparation method and application thereof
CN113004457A
Control over carboxyl group concentration of emulsion particle
JP1998120709A