Photo-initiated resin composition as well as preparation method and application thereof

By adding non-reactive silicone to the 3D printed resin composition, the problems of high resin viscosity and filler precipitation are solved, the characteristics of low viscosity and easy separation are achieved, printing efficiency and accuracy are improved, and the industry suitable for dental models is suitable for dentistry models. Scale application.

CN119060249AActive Publication Date: 2024-12-03GUANGZHOU HEIGE ZHIZAO INFORMATION TECH CO LTD

Patent Information

Application Number
CN202411374810.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-03
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

The existing 3D printed resin compositions used in dental models have too high viscosity, making them difficult to separate after curing, and filler precipitation may occur during preparation and application, affecting the printing quality and large-scale use.

Method used

By using the preparation method of the photoinitiating resin composition, a low viscosity, no precipitation resin composition is prepared by mixing acrylate monomer, photoinitiator and non-reactive silicone, adjusting the component ratio and stirring conditions, and non-reactive resin composition is prepared. The viscous silicone not only reduces the viscosity of the resin, but also makes it easy to separate from the mold after curing.

Benefits of technology

It realizes a resin composition that is free of precipitation, low viscosity, and easy to separate after curing, improves printing efficiency and accuracy, reduces the adhesion between the resin and the mold after curing, simplifies the separation process, and is suitable for industrial-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068415420000021
    Figure BDA0005068415420000021
  • Figure BDA0005068415420000031
    Figure BDA0005068415420000031
  • Figure BDA0005068415420000051
    Figure BDA0005068415420000051
Patent Text Reader

Abstract

The invention provides a photo-initiation resin composition as well as a preparation method and application thereof. The preparation method of the photo-initiation resin composition comprises the following steps: S1, mixing an acrylate monomer and a photoinitiator, and carrying out first stirring to obtain a first mixture; and S2, adding non-reactive organic silicon into the first mixture, and carrying out second stirring to obtain the resin composition, the photoinitiator is prepared from the following components in parts by weight: 30 to 70 parts of acrylate monomer, 1 to 5 parts of photoinitiator and 5 to 35 parts of non-reactive organic silicon. According to the present invention, with the well-designed composition formula and the well-designed preparation process, the preparation of the resin composition with characteristics of no precipitation, low viscosity and easy stripping from various interfaces after curing is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of resins for 3D printing, and in particular to a photoinitiator resin composition, a preparation method thereof and applications thereof. Background Art

[0002] For orthodontic applications, traditional processing plants use plaster casting to process and produce. Taking braces as an example, workers need to evenly apply a layer of release agent on the plaster model so that the braces solidified on it can be separated from the plaster model.

[0003] At present, it is common to use 3D printing technology to produce dental products, such as dental molds. When using the existing process of separating the orthodontic appliance, it is still necessary to apply a separating agent on the dental mold to facilitate the separation of the orthodontic appliance from the dental mold. There are currently 3D printing model resins that can be directly separated without applying a separating agent, but in this resin composition, for the purpose of ease of use, color-developing fillers, such as titanium dioxide, will inevitably be added to make the final cured resin model present a plaster-like white color, and the filler will precipitate during the storage process of the 3D printing model resin, which will not only affect the printing quality, but also require an additional step of shaking in advance, which is not suitable for large-scale use.

[0004] Based on this, how to provide a new resin composition that has both the characteristics of being separable without the use of a release agent after curing and the characteristics of being low-viscosity and having no precipitation is one of the important technical problems that need to be solved in this field. Summary of the invention

[0005] The main purpose of the present invention is to provide a photoinitiated resin composition, a preparation method and application thereof, so as to solve the problems in the prior art that the resin composition used for 3D printing dental models has high viscosity, is difficult to separate after curing, and may cause filler precipitation during the preparation and application process.

[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing a photoinitiator resin composition, comprising: step S1, mixing an acrylate monomer and a photoinitiator, and obtaining a first mixture after a first stirring; step S2, adding a non-reactive silicone to the first mixture, and obtaining a resin composition after a second stirring; in parts by weight, the acrylate monomer is 30 parts to 70 parts, the photoinitiator is 1 part to 5 parts, and the non-reactive silicone is 5 parts to 35 parts.

[0007] In certain embodiments, the non-reactive silicone is a linear polysilane, and the linear polysilane has a structure shown in Formula I:

[0008]

[0009] Wherein, R and R' are each independently a combination of one or more of hydrogen, C1-C6 alkyl, C1-C6 alkoxy, phenyl, phenoxy, C1-C6 alkyl-substituted phenyl and C1-C6 alkyl-substituted phenoxy, and n is any integer from 50 to 1200; preferably, R is methyl or p-methylphenyl, R' is hydrogen, and n is any integer from 200 to 800.

[0010] In certain embodiments, the non-reactive silicone is: wherein n is 600; and / or,

[0011] Where n is 600.

[0012] In certain embodiments, the acrylate monomer is selected from one or more of alkyl (meth)acrylate, hydroxy (meth)acrylate, (meth)acrylate with aromatic ring and / or aliphatic ring, glycol diacrylate, alkoxylated acrylate, dioxol acrylate and alkoxylated bisphenol A di(meth)acrylate, preferably acrylate monomer is selected from acryloyl morpholine, methacryloyl morpholine, cyclotrimethylolpropane formal acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, dicyclopentene acrylate, tetrahydrofurfuryl acrylate, acrylate monomer ... Acid ester, lauric acid acrylate, 2-phenoxyethyl methacrylate, 3,3,5-trimethylcyclohexane methacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (400) diacrylate, polyethylene glycol (600) diacrylate, 1,4-butanediol diacrylate, 1,6-dihexane diol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, (2-hydroxyethyl) isocyanuric acid triacrylate, isobornyl acrylate and isobornyl methacrylate; and / or, the photoinitiator is a free radical photoinitiator; preferably, the photoinitiator is selected from benzoyl formate, 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, phenyl bis (2 ,4,6-trimethylbenzoyl), ethyl 2,4,6-trimethylbenzoylphenylphosphonate, diphenyl ethyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, α,α'-dimethylbenzil ketal, α,α-diethoxyacetophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinoacetone-1 and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1 or more thereof.

[0013] In some embodiments, the first stirring is performed at a stirring speed of 600 r / min to 800 r / min, and the time is 20 min to 30 min; and / or the second stirring is performed at a stirring speed of 800 r / min to 1000 r / min, and the time is 20 min to 30 min.

[0014] In some embodiments, step S2 further includes adding a pigment to the first mixture, and obtaining a resin composition after a second stirring; preferably, the pigment includes one or more of complex blue, pigment red, carbon black, pigment yellow and pigment violet, and the pigment is 0.5 to 1.0 parts by weight.

[0015] In some embodiments, step S2 further includes adding 15 to 40 parts of acrylate oligomer to the first mixture.

[0016] In certain embodiments, by weight percentage, in the resin composition, the acrylate monomer is 30% to 70%, the photoinitiator is 1% to 5%, the non-reactive silicone is 5% to 35%, and the acrylate oligomer is 15% to 40%.

[0017] The second aspect of the present invention provides a photoinitiator resin composition, which is prepared by the above-mentioned method for preparing the photoinitiator resin composition; or, by weight, the resin composition comprises 30 to 70 parts of acrylate monomers, 1 to 5 parts of photoinitiators, and 5 to 35 parts of non-reactive silicones; preferably, the non-reactive silicone is a linear polysilane, and the linear polysilane has a structure shown in Formula I:

[0018]

[0019] wherein R and R' are independently selected from one or more of hydrogen, C1-C6 alkyl, C1-C6 alkoxy, phenyl, phenoxy, C1-C6 alkyl-substituted phenyl and C1-C6 alkyl-substituted phenoxy, and n is any integer from 50 to 1200; and / or, the acrylate monomer is selected from one or more of (meth) acrylate alkyl, (meth) acrylate hydroxy ester, (meth) acrylate with aromatic ring and / or aliphatic ring, glycol diacrylate, alkoxylated acrylate, dioxolyl acrylate and alkoxylated bisphenol A di(meth)acrylate; preferably, the acrylate monomer is selected from acryloyl morpholine, methacryloyl morpholine, cyclotrihydroxymethyl Propane methylal acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, dicyclopentene acrylate, tetrahydrofurfuryl acrylate, lauric acid acrylate, 2-phenoxyethyl methacrylate, 3,3,5-trimethylcyclohexane methacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (400) diacrylate, polyethylene glycol (600) diacrylate, 1,4-butanediol diacrylate, 1,6-dihexanediol diacrylate , dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, (2-hydroxyethyl) isocyanuric acid triacrylate, isobornyl acrylate and isobornyl methacrylate; and / or, the photoinitiator is a free radical photoinitiator, preferably the photoinitiator is selected from benzoyl formate, 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, phenyl bis (2,4,6-trimethylbenzoyl), ethyl 2,4,6-trimethylbenzoyl phenylphosphonate, dibenzoyl ethyl ketone, 2-hydroxy-2-methyl-1-phenyl-1 -acetone, 1-hydroxycyclohexyl phenyl ketone, α,α'-dimethylbenzil ketal, α,α-diethoxyacetophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholine acetone-1 and 2-benzyl-2-dimethylamino-1-(4-morpholine phenyl) butanone-1 or more; preferably, the resin composition also includes 15 to 40 parts of acrylate oligomers; more preferably, in the resin composition, by weight percentage, the acrylate monomer is 30% to 70%, the photoinitiator is 1% to 5%, the non-reactive silicone is 5% to 35%, and the acrylate oligomer is 15% to 40%.

[0020] In some embodiments, the viscosity of the photoinitiator resin composition at 25° C. is 180 mPa·s to 300 mPa·s. The short beam shear bonding strength of the resin obtained after the photoinitiator resin composition is photocured is 1.2 MPa to 1.9 MPa.

[0021] A third aspect of the present invention provides an application of the above-mentioned photoinitiator resin composition as a dental model resin composition for 3D printing to prepare a dental model.

[0022] In certain embodiments, a photoinitiator resin composition is 3D printed to obtain a 3D printed dental model, and then the 3D printed dental model is powdered to manufacture a dental product; preferably, the powdering comprises: step A, waxing and filling the undercuts on the cured 3D printed dental model to obtain a first product; step B, powdering the first product by a droplet method, and setting a retainer and / or a jaw pad on the first product to obtain a second product; step C, treating the second product at 0.1MPa to 0.3MPa and 40°C to 50°C for 10min to 20min to obtain a third product; step D, placing the third product at 20°C to 30°C for 5min to 15min, and then removing the retainer and / or jaw pad set thereon to obtain a dental product.

[0023] By applying the technical solution of the present invention, a resin composition with no precipitation, low viscosity, and easy peeling from various interfaces after curing is prepared through a carefully designed composition formula and preparation process. The addition of non-reactive silicone not only makes the resin composition appear white, but also reduces the viscosity of the resin composition, improves its fluidity, and effectively reduces the adhesion between the cured resin model and the mold, making the separation and treatment of the cured resin more convenient. DETAILED DESCRIPTION

[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0025] As described in the background art, the resin composition used for 3D printing dental models in the prior art has the problems of high viscosity, difficulty in separation after curing, and filler precipitation may occur during preparation and application. In order to solve the above technical problems, the first aspect of the present invention provides a method for preparing a photoinitiator resin composition, comprising: step S1, mixing an acrylate monomer and a photoinitiator, and obtaining a first mixture after a first stirring; step S2, adding a non-reactive silicone to the first mixture, and obtaining a resin composition after a second stirring; in parts by weight, the acrylate monomer is 30 to 70 parts, the photoinitiator is 1 to 5 parts, and the non-reactive silicone is 5 to 35 parts. For example, the acrylate monomer is 35 parts, the photoinitiator is 2 parts, and the non-reactive silicone is 10 parts. For example, the acrylate monomer is 50 parts, the photoinitiator is 3 parts, and the non-reactive silicone is 15 parts. For example, the acrylate monomer is 60 parts, the photoinitiator is 4 parts, and the non-reactive silicone is 20 parts. For another example, the acrylate monomer is 65 parts, the photoinitiator is 5 parts, and the non-reactive silicone is 30 parts.

[0026] The above preparation method realizes the preparation of a resin composition with no precipitation, low viscosity, and easy to peel from various interfaces after curing through a carefully designed composition formula and preparation process. In particular, in the prior art, in order to make the final cured resin present a plaster-like white color, it is inevitable to add color fillers such as titanium dioxide thereto, and the fillers will produce precipitation during the storage process of the 3D printing model resin, which will not only affect the printing quality, but also require the addition of a pre-shaking process, which is not suitable for large-scale use. The present invention creatively adds non-reactive silicone to the composition, first of all, it is not necessary to add additional white slurry fillers to achieve the white effect, and because there is no white slurry filler added, there is no problem of white slurry filler sinking to the bottom. At the same time, the addition of non-reactive silicone also significantly reduces the viscosity of the resin composition, improves its fluidity, and can improve the printing efficiency in 3D printing. More importantly, due to the lower viscosity, it is easier to clean the low-viscosity resin attached to the surface of the dental mold more cleanly. And, because the structure and chemical properties of non-reactive silicone are more stable, it will not destroy the resin structure obtained by the resin composition after curing, so that the printing accuracy and the mechanical properties of the cured resin can be better protected.

[0027] Specifically, in the above preparation method, the photoinitiator is first dissolved in the acrylate monomer, and then the non-reactive silicone is uniformly mixed in the mixture formed by the acrylate monomer and the photoinitiator through step S2. Compared with the method of adding all components at once and mixing and stirring, the above addition preparation method can improve the mixing uniformity between the components, especially more effectively promote the dispersion of the non-reactive silicone in the system, so as to prepare a resin composition with good comprehensive performance, especially lower viscosity, lower surface energy after curing, and easier separation from various surfaces.

[0028] At the same time, in order to better exert the synergistic effect between the components, the inventors have optimized the dosage of each component as above after a large number of experiments, and thus obtained a resin composition with lower viscosity, better fluidity, and easier peeling after curing.

[0029] In several typical embodiments, the non-reactive silicone is a linear polysilane, and the linear polysilane has a structure shown in Formula I:

[0030]

[0031] Wherein, R and R' are independently hydrogen, C1-C6 alkyl, C1-C6 alkoxy, phenyl, phenoxy, C1-C6 alkyl-substituted phenyl and C1-C6 alkyl-substituted phenoxy, and n is any integer from 50 to 1200, for example, n is 80, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000; preferably, R is methyl or p-methylphenyl, R' is hydrogen, and n is any integer from 200 to 800, for example, n is 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750. The inventors designed the types and structures of non-reactive silicone through a large number of experiments, and finally preferably obtained the above structure that can make the viscosity of the resin composition lower.

[0032] In practical applications, R can also be a combination of one or more of C1-C6 alkenyl, hydroxyl, acetoxy, chlorine, hydrogen, C1-C6 alkyl, phenyl, and C1-C6 alkyl-substituted phenyl; R' can also be a combination of one or more of ether bond, hydrogen, C1-C6 alkyl, phenyl, and C1-C6 alkyl-substituted phenyl. When the non-reactive silicone with the above structure is used as one of the components of the resin composition, the obtained resin composition can also exhibit the characteristics of low viscosity and easy separation after curing.

[0033] In some embodiments, R is methyl or p-methylphenyl, R' is hydrogen, and n is any integer between 200 and 800, for example, n is 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750. Adding the non-reactive silicone having the above structure as one of the components into the resin composition can more effectively reduce its viscosity and the surface energy of the cured resin, thereby obtaining a model resin product that is easier to separate from the mold.

[0034] In several more typical embodiments, in order to further reduce the viscosity of the obtained resin composition, improve the ease of stripping of the obtained resin after curing, and also make the non-reactive silicone more compatible with other components in the resin composition formula and be diluted, so as to improve the comprehensive performance of the resin composition, the inventors have preferably selected it after a large number of experiments: wherein n is 600; and / or, Where n is 600.

[0035] In certain embodiments, the acrylate monomer is selected from one or more of alkyl (meth)acrylate, hydroxy (meth)acrylate, (meth)acrylate with aromatic ring and / or aliphatic ring, glycol diacrylate, alkoxylated acrylate, dioxol acrylate and alkoxylated bisphenol A di(meth)acrylate, preferably acrylate monomer is selected from acryloyl morpholine, methacryloyl morpholine, cyclotrimethylolpropane formal acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, dicyclopentene acrylate, tetrahydrofurfuryl acrylate, lauric acid acrylate, 2-phenoxyethyl methacrylate, 3,3,5-trimethylcyclohexane methacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane Dimethylol dimethacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (400) diacrylate, polyethylene glycol (600) diacrylate, 1,4-butanediol diacrylate, 1,6-dihexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, (2-hydroxyethyl) isocyanuric acid triacrylate, isobornyl acrylate and isobornyl methacrylate. The selection of the above monomers further improves the resin composition after light curing, and the resulting resin has better structural properties and mechanical strength.

[0036] In practical applications, in addition to the above types, the acrylate monomer can also be selected from lauryl acrylate, glycidyl methacrylate, tetrahydrofuran methyl acrylate, phenoxyethyl acrylate and phenoxyethyl methacrylate.

[0037] And / or, the photoinitiator is a free radical photoinitiator; preferably, the photoinitiator is selected from one or more of benzoyl formate, 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, phenyl bis (2,4,6-trimethylbenzoyl), 2,4,6-trimethylbenzoyl phenylphosphonate, diphenyl ethyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, α, α'-dimethylbenzil ketal, α, α-diethoxyacetophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinoacetone-1 and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl) butanone-1. The selection of the above-mentioned photoinitiator optimizes the curing speed and curing wavelength of the resin composition, so that it can be better applied to various 3D printing equipment and realize a fast and efficient curing process.

[0038] And, in practical applications, in addition to the above types, the photoinitiator can also be selected from other types of benzoin and its derivatives, benzil and its derivatives, acetophenone derivatives, α-hydroxyketone derivatives, α-aminoketone derivatives, benzoylformates and acylphosphine oxides.

[0039] In several typical embodiments, the stirring speed of the first stirring is 600 r / min to 800 r / min, and the time is 20 min to 30 min. The inventors have optimized the mixing conditions of the acrylate monomer and the photoinitiator through a large number of experiments, and found that the above stirring conditions can better promote the uniform mixing of the two, more effectively avoid inconsistent curing due to uneven mixing, or prepolymerization due to too intense mixing conditions, so as to more significantly improve the performance of the resin composition during preparation and after curing.

[0040] In some embodiments, adapted to the above-mentioned first stirring conditions, the inventors further preferred, through a large number of experiments, that the second stirring speed be 800 r / min to 1000 r / min, and the time be 20 min to 30 min. Such a stirring speed can further improve the dispersion uniformity of the components in the resin composition, especially the dispersion degree of the non-reactive silicone therein, thereby obtaining a resin composition with lower viscosity and easier separation from various surfaces after curing.

[0041] In several typical embodiments, step S2 further includes adding a pigment to the first mixture, and obtaining a resin composition after a second stirring, so as to obtain a resin composition with lower surface energy after curing, or better antibacterial property, or better able to meet color requirements. Preferably, the pigment includes one or more of complex blue, pigment red, carbon black, pigment yellow and pigment violet, which can be dissolved in the resin composition provided by the present invention without precipitation, and play a good color development role, and the pigment is 0.5 to 1.0 parts by weight, such as 0.6 parts, 0.7 parts, 0.8 parts, and 0.9 parts.

[0042] In some embodiments, step S2 further includes adding 15 to 40 parts of an acrylate oligomer to the first mixture, such as 20 parts, 25 parts, 30 parts, or 35 parts, so as to significantly improve the peeling and molding stability of the resin composition after curing. It is further preferred that the acrylate oligomer is selected from one or more of Sartomer SR991, Dymax BR970, and Sartomer SR996. In theory, the type and specific model of the acrylate oligomer can be selected from the types commonly used in this field or similar fields, and the above-mentioned models selected by the inventors through a large number of experiments can be better adapted to the above-mentioned resin composition system, thereby obtaining a resin composition with better dispersion uniformity, lower viscosity, easier peeling and separation after curing, and better mechanical properties.

[0043] In certain embodiments, in the resin composition, by weight percentage, the acrylate monomer is 30% to 70%, the photoinitiator is 1% to 5%, the non-reactive silicone is 5% to 35%, and the acrylate oligomer is 15% to 40%. This content ratio relationship and formula design can obtain a resin composition with better comprehensive performance after curing. For example, the acrylate monomer is 68%, the photoinitiator is 2%, the non-reactive silicone is 10%, and the acrylate oligomer is 20%. For example, the acrylate monomer is 57%, the photoinitiator is 3%, the non-reactive silicone is 15%, and the acrylate oligomer is 25%. For example, the acrylate monomer is 46%, the photoinitiator is 4%, the non-reactive silicone is 20%, and the acrylate oligomer is 30%. For another example, the acrylate monomer is 30%, the photoinitiator is 5%, the non-reactive silicone is 30%, and the acrylate oligomer is 35%.

[0044] Furthermore, in practical applications, ester compounds may be added thereto to help increase the curing speed and surface finish of the resin composition, thereby making the surface of the printed model resin smoother.

[0045] The second aspect of the present invention provides a photoinitiator resin composition, which is prepared by the above-mentioned method for preparing the photoinitiator resin composition; or, by weight, the resin composition comprises 30 to 70 parts of acrylate monomers, 1 to 5 parts of photoinitiators, and 5 to 35 parts of non-reactive silicones; preferably, the non-reactive silicone is a linear polysilane, and the linear polysilane has a structure shown in Formula I:

[0046]

[0047] wherein R and R' are independently a combination of one or more of hydrogen, C1-C6 alkyl, C1-C6 alkoxy, phenyl, phenoxy, C1-C6 alkyl-substituted phenyl and C1-C6 alkyl-substituted phenoxy, and n is any integer from 50 to 1200; and / or, the acrylate monomer is selected from one or more of (meth) acrylate alkyl, (meth) acrylate hydroxy ester, (meth) acrylate with aromatic ring and / or aliphatic ring, glycol diacrylate, alkoxylated acrylate, dioxolyl acrylate and alkoxylated bisphenol A di(meth)acrylate; preferably, the acrylate monomer is selected from acryloyl morpholine, methacryloyl morpholine cyclotrimethylolpropane formal acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, dicyclopentene acrylate, tetrahydrofurfuryl acrylate, lauric acid acrylate, 2-phenoxyethyl methacrylate, 3,3,5-trimethylcyclohexane methacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (400) diacrylate, polyethylene glycol (600) diacrylate, 1,4-butanediol diacrylate , 1,6-dihexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, (2-hydroxyethyl) isocyanuric acid triacrylate, isobornyl acrylate and isobornyl methacrylate; and / or, the photoinitiator is a free radical photoinitiator, preferably the photoinitiator is selected from benzoyl formate, 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, phenyl bis (2,4,6-trimethylbenzoyl), 2,4,6-trimethylbenzoyl phenylphosphonic acid ethyl ester, diphenyl One or more of ethanol ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, α,α'-dimethylbenzil ketal, α,α-diethoxyacetophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinoacetone-1 and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1; preferably, the resin composition further comprises 15 to 40 parts of an acrylate oligomer; further preferably, the acrylate oligomer is selected from one or more of Sartomer SR991, Dymax BR970 and Sartomer SR996.

[0048] In certain embodiments, by weight percentage, in the resin composition, the acrylate monomer is 30% to 70%, the photoinitiator is 1% to 5%, the non-reactive silicone is 5% to 35%, and the acrylate oligomer is 15% to 40%.

[0049] The obtained resin composition has lower viscosity and better fluidity, which is more conducive to improving the surface accuracy after curing. At the same time, the resin obtained by the resin composition after curing can be separated from the mold or any surface without any separating agent.

[0050] In certain embodiments, the viscosity of the photoinitiator resin composition at 25° C. is 180 mPa·s to 300 mPa·s, and the short beam shear bond strength of the resin obtained after the photoinitiator resin composition is photocured is 1.2 MPa to 1.9 MPa. That is, the viscosity of the obtained resin composition is lower, and the resin obtained after photocuring is also easier to separate from the surface on which it is located.

[0051] The third aspect of the present invention provides an application of the above-mentioned photoinitiator resin composition as a dental model resin composition for 3D printing. The obtained resin composition has low viscosity, is easy to separate after curing, and does not cause filler precipitation and other problems during the preparation and application process. Therefore, it is suitable for the preparation of 3D printed dental models, and exhibits higher printing efficiency and printing accuracy during the 3D printing process. At the same time, it is easier to separate from the surface, and the post-processing is more convenient, and it is also more suitable for large-scale industrial applications.

[0052] In certain embodiments, a photoinitiator resin composition is 3D printed to obtain a 3D printed dental model, and then the 3D printed dental model is sequentially cleaned, cured and powdered to obtain a dental model; preferably, powdering comprises: step A, waxing and filling undercuts on the cured 3D printed dental model to obtain a first product; step B, powdering the first product by a droplet method, and setting a retainer and / or a jaw pad on the first product to obtain a second product; step C, treating the second product at 0.1MPa~0.3MPa and 40℃~50℃ for 10min~20min to obtain a third product; step D, placing the third product at 20℃~30℃ for 5min~15min, and then removing the retainer and / or jaw pad set thereon to obtain a dental model.

[0053] In a specific dental model manufacturing process, the photoinitiator resin composition is poured into a material tray of a 3D printer for printing to obtain a 3D printed dental model, and then cleaned within 12 hours according to the steps and parameters in the following table.

[0054] Cleaning solvent Cleaning method Isopropyl alcohol 2min (rough wash) + blowing 30S + 1min (fine wash) + blowing 30S 95% medical alcohol 1min (rough wash) + blowing 30S + 1min (fine wash) + blowing 30S 75% medical alcohol 1min (rough wash) + blowing 30S + 1min (fine wash) + blowing 30S

[0055] The cleaned model is cured, and then the treated 3D printed dental model is powdered with self-curing resin, and finally a dental model that meets the use requirements is obtained. When powdering, the model obtained by 3D printing is first surrounded by wax and filled with undercuts, which means filling the undercuts on the tooth model (i.e., the sunken part on the tooth model); then the model is powdered using the drip method, retainers and / or jaw pads are made, and the retainers and / or jaw pads are set on the powdered model; then the powdered model with retainers and / or jaw pads is placed in a pressure cooker with an air pressure of 0.2MPa (the water in the pot needs to completely immerse the model), and boiled at 45°C for 15 minutes; then, the obtained model is placed at room temperature for 10 minutes, and after cooling to room temperature, the retainers and / or jaw pads on the model are removed with tools (such as wax knives).

[0056] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0057] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0058] Example 1

[0059] A method for preparing a photoinitiator resin composition:

[0060] Based on the total weight of the photoinitiator resin composition as 100%, the ingredients are formulated as follows: dipropylene glycol diacrylate (acrylate monomer): 58%; ethyl acrylate oligomer Sartomer SR991: 30%; non-reactive silicone: 10%; 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide (photoinitiator): 2%.

[0061] The structural formula of non-reactive silicone is: n is 600.

[0062] Step S1: stirring a mixture of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide and dipropylene glycol diacrylate at a rotation speed of 700 r / min for 25 min to completely dissolve 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, thereby obtaining a first mixture;

[0063] Step S2: Continue to add acrylate oligomer and non-reactive silicone to the first mixture, and continue stirring at a speed of 900 r / min for 25 minutes to obtain a photoinitiator resin composition.

[0064] The resulting composition exhibits white color after curing.

[0065] Example 2

[0066] A method for preparing a photoinitiator resin composition:

[0067] The only difference between this embodiment and embodiment 1 is that in step S2, 0.5% of complex blue is further added as a pigment, and the amount of dipropylene glycol diacrylate is correspondingly reduced to 47.5%.

[0068] The resulting composition exhibited a blue color after curing.

[0069] Example 3

[0070] A method for preparing a photoinitiator resin composition:

[0071] The difference between this embodiment and embodiment 1 is that another non-reactive silicone of equal weight is used to replace the original non-reactive silicone in embodiment 1. The structural formula of the other non-reactive silicone is:

[0072] n is 600.

[0073] Example 4

[0074] A method for preparing a photoinitiator resin composition:

[0075] The difference between this embodiment and embodiment 1 is that the rotation speed in step S1 is changed to 600 r / min and the time is changed to 30 min; the rotation speed in step S2 is changed to 1000 r / min and the time is changed to 20 min.

[0076] Example 5

[0077] A method for preparing a photoinitiator resin composition:

[0078] The difference between this embodiment and embodiment 1 is that the speed in step S1 is changed to 800 r / min and the time is changed to 20 min; the speed in step S2 is changed to 800 r / min and the time is changed to 30 min.

[0079] Example 6

[0080] A method for preparing a photoinitiator resin composition:

[0081] The difference between this embodiment and embodiment 1 is that the speed in step S1 is changed to 500 r / min and the time is changed to 40 min; the speed in step S2 is changed to 1200 r / min and the time is changed to 10 min.

[0082] Example 7

[0083] A method for preparing a photoinitiator resin composition:

[0084] The difference between this embodiment and embodiment 1 is that the rotation speed in step S1 is changed to 900 r / min and the time is changed to 10 min; the rotation speed in step S2 is changed to 600 r / min and the time is changed to 40 min.

[0085] Example 8

[0086] A method for preparing a photoinitiator resin composition:

[0087] The only difference between this embodiment and embodiment 1 is that the type of acrylate monomer is changed to acryloylmorpholine, the type of photoinitiator is changed to 2-hydroxy-2-methyl-1-phenyl-1-propanone, the type of acrylate oligomer is changed to Sartomer SR996, and other conditions and parameters remain unchanged.

[0088] Example 9

[0089] A method for preparing a photoinitiator resin composition:

[0090] The only difference between this embodiment and embodiment 1 is that the type of acrylate monomer is changed to trimethylolpropane triacrylate, the type of photoinitiator is changed to 1-hydroxycyclohexyl phenyl ketone, the type of acrylate oligomer is changed to Dymax BR970, and other parameters remain unchanged.

[0091] Comparative Example 1

[0092] A method for preparing a photoinitiator resin composition:

[0093] The only difference between this comparative example and Example 1 is that non-reactive silicone is not added, and the amounts of other components are adjusted accordingly: dipropylene glycol diacrylate: 63%; ethyl acrylate oligomer Sartomer SR991: 35%; 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide (photoinitiator): 2%.

[0094] The obtained resin composition is transparent after curing and is difficult to be used in practical applications.

[0095] Comparative Example 2

[0096] A method for preparing a photoinitiator resin composition:

[0097] The difference between this comparative example and Example 1 is that the amount of each component is different, specifically: based on the total weight of the photoinitiator resin composition as 100%, dipropylene glycol diacrylate: 35%; ethyl acrylate oligomer Sartomer SR991: 40%; non-reactive silicone: 24.0%; 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide: 0.5%; at the same time, in order to make the resin composition appear white after curing, 0.5% of titanium dioxide is added for the purpose of mixing.

[0098] Comparative Example 3

[0099] A method for preparing a photoinitiator resin composition:

[0100] The difference between this comparative example and Example 1 is that the amount of each component is different. Specifically, based on the total weight of the photoinitiator resin composition as 100%, the ingredients are prepared according to the following: dipropylene glycol diacrylate: 70%; ethyl acrylate oligomer Sartomer SR991: 18%; non-reactive silicone: 4%; 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide: 8%.

[0101] Comparative Example 4

[0102] A method for preparing a photoinitiator resin composition:

[0103] The difference between this comparative example and Example 1 is that the preparation method is different, specifically: a mixture of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, dipropylene glycol diacrylate, acrylate oligomer and non-reactive silicone is stirred at a rotation speed of 700 r / min for 25 minutes to directly obtain a photoinitiator resin composition.

[0104] That is, this comparative example does not have a two-step mixing method, but directly mixes and stirs all components in a one-step method to obtain the photoinitiator resin composition.

[0105] Comparative Example 5

[0106] A method for preparing a photoinitiator resin composition:

[0107] The only difference between this comparative example and Example 1 is that the non-reactive silicone in the components is replaced by an equal weight of a silane coupling agent, γ-aminopropyltriethoxysilane (KH-570).

[0108] The obtained resin composition is transparent after curing and is difficult to be used in practical applications.

[0109] Test Method

[0110] Viscosity of the photoinitiator resin composition: tested according to ASTM D2393-1986.

[0111] Whether the photoinitiator resin composition has precipitation problem: The test method is: pour the evenly mixed finished resin into a 100 ml test tube, place the test tube in an oven at 80°C and bake for 7 days. After 7 days, take out the test tube and observe with the naked eye whether there is precipitation at the bottom of the test tube.

[0112] Short beam shear bond strength: Referring to GB-T 30969-2014, the improved short beam shear bond strength test is used to measure the bond strength between the sample and the self-curing resin, so as to evaluate the "anti-adhesion ability" of the obtained photoinitiated resin composition to the dental self-curing resin after curing. Specifically, the test specimen is divided into two, one half is made of the resin composition by additive manufacturing printing and post-processing, placed in the mold, and the self-curing resin powder and liquid mixture are poured in. After the self-curing resin solidifies, the specimen is demolded from the mold. In particular, the bonding surface of the half-specimen printed by the model material is designed to be serrated, so as to increase the bonding area of ​​the two materials and improve the signal-to-noise ratio and confidence of the test results. The complete tensile specimen composed of the cured resin model material and the cured self-curing resin was placed in a dental high-pressure polymerization pot. After polymerization was completed under the conditions of 2 bar, 40°C, and 15 min, it was cooled to room temperature and kept warm for 5 min to 10 min. Then, loading and testing were completed on a universal testing machine using the equipment parameters specified in GB-T30969-2014, and the short beam shear bond strength was calculated.

[0113] The resin compositions obtained in the examples and comparative examples were tested as above, and the results are shown in Table 1.

[0114] Table 1

[0115] Is there precipitation? Viscosity at 25°C / mPa·s Short beam shear bond strength / MPa Example 1 no 200±20 1.328±0.20 Example 2 no 200±20 1.326±0.10 Example 3 no 230±20 1.310±0.15 Example 4 no 210±20 1.446±0.10 Example 5 no 200±20 1.502±0.20 Example 6 no 270±20 1.838±0.40 Example 7 no 250±20 1.663±0.35 Example 8 no 220±20 1.457±0.15 Example 9 no 210±20 1.326±0.40 Comparative Example 1 no 310±20 13.269±0.42 Comparative Example 2 have 210±20 6.336±0.50 Comparative Example 3 no 300±20 11.215±0.20 Comparative Example 4 no 200±20 15.162±0.18 Comparative Example 5 no 230±20 13.429±0.32

[0116] From the above description, it can be seen that the above embodiments of the present invention achieve the preparation of a resin composition with low viscosity, high fluidity, no precipitation, and the resin obtained after curing is easy to separate.

[0117] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0118] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a photoinitiator resin composition, characterized in that: The preparation method of the photoinitiator resin composition comprises: Step S1, mixing an acrylate monomer and a photoinitiator, and obtaining a first mixture after a first stirring; Step S2, adding non-reactive silicone to the first mixture, and obtaining the resin composition after a second stirring; In parts by weight, the acrylate monomer is 30 to 70 parts, the photoinitiator is 1 to 5 parts, and the non-reactive silicone is 5 to 35 parts.

2. The method for preparing the photoinitiator resin composition according to claim 1, characterized in that: The non-reactive organosilicon is a linear polysilane, and the linear polysilane has a structure shown in Formula I: wherein R and R' are each independently a combination of one or more of hydrogen, C1-C6 alkyl, C1-C6 alkoxy, phenyl, phenoxy, C1-C6 alkyl-substituted phenyl and C1-C6 alkyl-substituted phenoxy, and n is any integer from 50 to 1200; Preferably, R is methyl or p-methylphenyl, R' is hydrogen, and n is any integer between 200 and 800.

3. The method for preparing the photoinitiator resin composition according to claim 1 or 2, characterized in that: The non-reactive silicone is: wherein n is 600; and / or, Where n is 600.

4. The method for preparing a photoinitiator resin composition according to any one of claims 1 to 3, characterized in that: The acrylate monomer is selected from one or more of alkyl (meth)acrylate, hydroxy (meth)acrylate, (meth)acrylate with aromatic ring and / or aliphatic ring, glycol diacrylate, alkoxylated acrylate, dioxol acrylate and alkoxylated bisphenol A di(meth)acrylate; preferably, the acrylate monomer is selected from acryloyl morpholine, methacryloyl morpholine, cyclotrimethylolpropane formal acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, dicyclopentene acrylate, tetrahydrofurfuryl acrylate, lauric acid acrylate, 2-phenoxyethyl methacrylate, 3,3,5-trimethylcyclohexane methacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol diacrylate, methacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (400) diacrylate, polyethylene glycol (600) diacrylate, 1,4-butanediol diacrylate, 1,6-dihexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, (2-hydroxyethyl) isocyanuric acid triacrylate, isobornyl acrylate and isobornyl methacrylate; and / or, The photoinitiator is a free radical photoinitiator, and preferably the photoinitiator is selected from one or more of benzoylformate, 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, phenyl bis (2,4,6-trimethylbenzoyl), 2,4,6-trimethylbenzoyl phenylphosphonate, diphenyl ethyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, α, α'-dimethylbenzil ketal, α, α-diethoxyacetophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinoacetone-1 and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl) butanone-1.

5. The method for preparing the photoinitiator resin composition according to any one of claims 1 to 4, characterized in that: The first stirring has a stirring speed of 600 r / min to 800 r / min and a time of 20 min to 30 min; and / or, The second stirring is performed at a stirring speed of 800 r / min to 1000 r / min, and the stirring time is 20 min to 30 min.

6. The method for preparing a photoinitiator resin composition according to any one of claims 1 to 5, characterized in that: Step S2 further includes adding a pigment into the first mixture, and obtaining the resin composition after the second stirring; Preferably, the pigment includes one or more of complex blue, pigment red, carbon black, pigment yellow and pigment violet, and the pigment is 0.5 to 1.0 parts by weight.

7. The method for preparing a photoinitiator resin composition according to any one of claims 1 to 6, characterized in that: Step S2 further includes adding 15 to 40 parts of acrylate oligomer to the first mixture.

8. The method for preparing the photoinitiator resin composition according to claim 7, characterized in that: In terms of weight percentage, in the resin composition, the acrylate monomer accounts for 30% to 70%, the photoinitiator accounts for 1% to 5%, the non-reactive silicone accounts for 5% to 35%, and the acrylate oligomer accounts for 15% to 40%.

9. A photoinitiator resin composition, characterized in that: The resin composition is prepared by the method for preparing a photoinitiator resin composition according to any one of claims 1 to 8; or, by weight, the resin composition comprises 30 to 70 parts of acrylate monomers, 1 to 5 parts of photoinitiators, and 5 to 35 parts of non-reactive silicones; Preferably, the non-reactive organosilicon is a linear polysilane, and the linear polysilane has a structure shown in Formula I: wherein R and R' are each independently a combination of one or more of hydrogen, C1-C6 alkyl, C1-C6 alkoxy, phenyl, phenoxy, C1-C6 alkyl-substituted phenyl and C1-C6 alkyl-substituted phenoxy, and n is any integer from 50 to 1200; and / or, The acrylate monomer is selected from one or more of alkyl (meth)acrylate, hydroxy (meth)acrylate, (meth)acrylate with aromatic ring and / or aliphatic ring, glycol diacrylate, alkoxylated acrylate, dioxol acrylate and alkoxylated bisphenol A di(meth)acrylate; preferably, the acrylate monomer is selected from acryloyl morpholine, methacryloyl morpholine, cyclotrimethylolpropane formal acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, dicyclopentene acrylate, tetrahydrofurfuryl acrylate, lauric acid acrylate, 2-phenoxyethyl methacrylate, 3,3,5-trimethylcyclohexane methacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol diacrylate, methacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (400) diacrylate, polyethylene glycol (600) diacrylate, 1,4-butanediol diacrylate, 1,6-dihexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, (2-hydroxyethyl) isocyanuric acid triacrylate, isobornyl acrylate and isobornyl methacrylate; and / or, The photoinitiator is a free radical photoinitiator, and preferably the photoinitiator is selected from one or more of benzoylformate, 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, phenyl bis (2,4,6-trimethylbenzoyl), 2,4,6-trimethylbenzoyl phenylphosphonate, diphenyl ethyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, α, α'-dimethylbenzil ketal, α, α-diethoxyacetophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinoacetone-1 and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl) butanone-1; Preferably, the resin composition further comprises 15 to 40 parts of an acrylate oligomer; More preferably, in the resin composition, by weight percentage, the acrylate monomer is 30% to 70%, the photoinitiator is 1% to 5%, the non-reactive silicone is 5% to 35%, and the acrylate oligomer is 15% to 40%.

10. The photoinitiator resin composition according to claim 9, characterized in that: The viscosity of the photoinitiator resin composition at 25° C. is 180 mPa·s to 300 mPa·s. The photoinitiator resin composition is photoinitiated and cured to obtain a resin, and the short beam shear bonding strength of the resin is 1.2 MPa to 1.9 MPa.

11. Use of the photoinitiator resin composition according to claim 9 or 10 as a dental model resin composition for 3D printing to prepare a dental model.

12. The use according to claim 11, characterized in that: The photoinitiator resin composition is 3D printed to obtain a 3D printed dental model, and then the 3D printed dental model is powdered to manufacture a dental product; Preferably, the powder spreading comprises: Step A, waxing and filling undercuts on the solidified 3D printed dental model to obtain a first product; Step B, spreading powder on the first product by a dropping method, and setting a retainer and / or a jaw pad on the first product to obtain a second product; Step C, treating the second product at 0.1 MPa to 0.3 MPa and 40° C. to 50° C. for 10 min to 20 min to obtain a third product; Step D: placing the third product at 20° C. to 30° C. for 5 to 15 minutes, and then removing the retainer and / or the jaw pad disposed thereon to obtain the dental product.

Citation Information

Patent Citations

  • 3D printing photosensitive resin material

    CN107868443A

  • High-toughness hybrid 3D printing light-cured resin and preparation method thereof

    CN113861355A

  • Organic light emitting device

    KR1020220145292A

  • UV curable composition for use in 3D printing

    US20210395558A1

Cited By

  • Photo-initiated resin composition, preparation method therefor, and use thereof

    WO2026067717A1