Modified diene polymer as well as preparation method and application thereof

A modified diene polymer with monovinyl aromatic and conjugated diene units and mercaptocarboxylic acid side chains addresses the compatibility issues of aromatic oils, improving rubber processing and performance by enhancing anti-skid and reducing rolling resistance.

CN119060252APending Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310637408.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing environmentally friendly aromatic oils fail to improve the processability of rubber and simultaneously enhance anti-skid performance and reduce rolling resistance due to compatibility issues with silica fillers, leading to precipitation and environmental pollution.

Method used

A modified diene polymer with a main chain containing monovinyl aromatic structural units and conjugated diene structural units, along with mercaptocarboxylic acid side chains, is introduced to improve affinity with silica and enhance anti-skid performance and reduce rolling resistance.

Benefits of technology

The modified diene polymer improves the affinity with white carbon black, enhancing the processing performance and achieving high anti-slip and low rolling resistance in rubber products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004260822100000051
    Figure BDA0004260822100000051
  • Figure BDA0004260822100000181
    Figure BDA0004260822100000181
  • Figure BDA0004260822100000191
    Figure BDA0004260822100000191
Patent Text Reader

Abstract

The invention relates to the technical field of rubber additives, and discloses a modified diene polymer as well as a preparation method and application thereof. The modified diene polymer comprises a main chain containing a monovinylarene structural unit and a conjugated diene structural unit and a mercapto carboxylic acid side chain suspended on the main chain, and the content of the mercapto carboxylic acid side chain is 1-10 wt% based on the total weight of the modified diene polymer; the general formula of the sulfydryl carboxylic acid side chain is-S-R-COOH. The modified diene polymer disclosed by the invention can be used as a rubber processing aid to be added into a rubber processing process, so that the affinity of the modified diene polymer with white carbon black and the processability of rubber can be improved, and the high wet skid resistance and low rolling resistance of a rubber product can be improved at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber additives, and in particular to a modified diene polymer and a preparation method and application thereof. Background Art

[0002] In recent years, with the development of the automobile industry and the rising oil prices, people are paying more and more attention to the safety and energy saving of automobiles, which requires tires to have high anti-skid performance and low rolling resistance. However, it is often difficult to improve anti-skid performance and reduce rolling resistance at the same time. Therefore, according to different usage requirements, it is necessary to find the best balance between high anti-skid performance and low rolling resistance.

[0003] For the production of low rolling resistance tires, anionic solution polymerization has a more significant advantage than emulsion polymerization of styrene butadiene because anionic solution polymerization can effectively adjust the content of conjugated diene structural units with double bonds in the side chains and the glass transition temperature. This advantage is beneficial for balancing the relationship between the tire's anti-skid performance and rolling resistance.

[0004] In addition, studies have shown that adding aromatic oil during the rubber mixing process can promote the dispersion of fillers in raw rubber to a certain extent and improve the relationship between the rubber's anti-skid performance and rolling resistance to a certain extent. However, traditional environmentally friendly aromatic oils are composed of a mixture of small molecules, which are difficult to be compatible with the polar silica filler. They are free in rubber products and are easy to precipitate, causing pollution to the atmosphere. In addition to improving the processability of the rubber mixing process, they have almost no contribution to the rubber's anti-skid performance and low rolling resistance.

[0005] Therefore, it is of great significance to research and develop a rubber processing aid that can be added to rubber, while meeting the requirements of rubber processing performance, having affinity with silica and preventing it from precipitating from the product, and at the same time meeting the requirements of rubber products for anti-slip properties and low rolling resistance. Summary of the invention

[0006] The purpose of the present invention is to overcome the problem that the environmentally friendly aromatic oil in the prior art cannot simultaneously improve the processability of rubber and effectively improve the anti-skid performance and rolling resistance of rubber, and to provide a modified diene polymer and a preparation method and application thereof. The modified diene polymer is used as a rubber additive. When added to rubber, the agglomeration problem of the rubber can be improved, and the requirements for the anti-skid performance and low rolling resistance performance of rubber products can be met at the same time.

[0007] In order to achieve the above object, the first aspect of the present invention provides a modified diene polymer, wherein the modified diene polymer comprises a main chain containing monovinyl aromatic structural units and conjugated diene structural units and a mercaptocarboxylic acid side chain suspended from the main chain, wherein the content of the mercaptocarboxylic acid side chain is 1-10wt% based on the total weight of the modified diene polymer; the general formula of the mercaptocarboxylic acid side chain is -SR-COOH, wherein R is selected from a linear or branched C1-C 10 Alkylene.

[0008] The second aspect of the present invention provides a method for preparing a modified diene polymer, the method comprising: in an inert atmosphere, in the presence of a first initiator, contacting a diene polymer containing a monovinyl aromatic hydrocarbon structural unit and a conjugated diene structural unit with a mercaptocarboxylic acid compound for reaction, wherein the contact conditions allow the mercaptocarboxylic acid compound to be chemically bonded to the diene polymer to form a mercaptocarboxylic acid side chain, thereby obtaining a modified diene polymer; based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chain is 1-10wt%; the general formula of the mercaptocarboxylic acid compound is HS-R-COOH, wherein R is selected from a linear or branched C1-C 10 Alkylene.

[0009] The third aspect of the present invention provides a modified diene polymer obtained by the aforementioned preparation method.

[0010] The fourth aspect of the present invention provides the use of the aforementioned modified diene polymer as a rubber processing aid in a rubber processing process.

[0011] The fifth aspect of the present invention provides a rubber composition, which contains rubber and the aforementioned modified diene polymer; wherein the amount of the modified diene polymer is 5-30 parts by weight based on 100 parts by weight of the rubber composition.

[0012] A sixth aspect of the present invention provides a vulcanized rubber obtained by vulcanizing the rubber composition described above.

[0013] A seventh aspect of the present invention provides use of the aforementioned rubber composition or the aforementioned vulcanized rubber in tire manufacturing or plastic modification, preferably in tire tread rubber.

[0014] Through the above technical scheme, the modified diene polymer and its preparation method and application provided by the present invention achieve the following beneficial effects:

[0015] (1) The modified diene polymer obtained by modifying the diene polymer with carboxylic acid functional groups can be added to the rubber processing process as a rubber processing aid, which can improve its affinity with white carbon black and the processing performance of rubber, and can also improve the high anti-slip and low rolling resistance performance of rubber products.

[0016] (2) The present invention modifies the diene polymer to give it a certain polarity, which can effectively increase its affinity with white carbon black, thereby improving some properties of rubber products. DETAILED DESCRIPTION

[0017] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0018] The first aspect of the present invention provides a modified diene polymer, the modified diene polymer comprising a main chain containing monovinyl aromatic structural units and conjugated diene structural units and a mercaptocarboxylic acid side chain suspended from the main chain, wherein, based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chain is 1-10wt%, for example, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% and any value in the range consisting of any two of the above values; the general formula of the mercaptocarboxylic acid side chain is -SR-COOH, wherein R is selected from a linear or branched C1-C 10 Alkylene.

[0019] In the present invention, the modified diene polymer comprises a main chain containing monovinyl aromatic structural units and conjugated diene structural units and mercaptocarboxylic acid side chains suspended from the main chain, and thus has a certain polarity.

[0020] In the present invention, the main chain of the modified diene polymer is a block copolymer.

[0021] In some embodiments of the present invention, R is selected from a linear or branched C1-C 10 The alkylene group is preferably a methylene group or an ethylene group.

[0022] In some embodiments of the present invention, based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chains is 2-5 wt %.

[0023] In the present invention, when the content of mercaptocarboxylic acid side chains meets the above range, the comprehensive dynamic properties of the modified diene polymer are further improved. When the content of mercaptocarboxylic acid side chains is 1-10wt%, the modified diene polymer has the advantage of being able to improve the comprehensive dynamic properties of rubber. When the content of mercaptocarboxylic acid side chains is less than 1wt%, too few polar groups are introduced to better affinity with white carbon black. When the content of mercaptocarboxylic acid side chains is greater than 10wt%, the rigidity of the modified diene polymer is too strong, which has a certain impact on the rubber processing process. Further, when the content of mercaptocarboxylic acid side chains is 2-5wt%, the comprehensive properties of the modified diene polymer are even better.

[0024] In some embodiments of the present invention, based on the total weight of the modified diene polymer, the content of the conjugated diene structural unit having a double bond in the side chain is 15-45 wt %, preferably 30-40 wt %.

[0025] In the present invention, the conjugated diene structural unit having a double bond in the side chain refers to a conjugated diene structural unit containing an unsaturated side group, and the unsaturated side group is provided by a conjugated diene monomer.

[0026] In the present invention, a nuclear magnetic resonance spectrometer ( 1 H-NMR) is used to analyze and test the content of mercaptocarboxylic acid side chains and the content of conjugated diene structural units containing double bonds in the side chains of the polymer. For example, the measurement can be performed using an AVANCE DRX 400MHz nuclear magnetic resonance spectrometer purchased from Bruker, Switzerland, wherein the solvent is deuterated chloroform. The specific measurement method is well known to those skilled in the art and will not be described in detail herein.

[0027] In some embodiments of the present invention, the coupling efficiency of the modified diene polymer is 50-95%, preferably 70-90%, and more preferably 80-90%.

[0028] In the present invention, the coupling efficiency is measured in weight percentage based on the total weight of the modified diene polymer.

[0029] In some embodiments of the present invention, based on the total weight of the modified diene polymer, the content of the monovinyl aromatic structural unit is 2-10wt%, preferably 3-6wt%; the content of the conjugated diene structural unit is 80-97wt%, preferably 89-95wt%.

[0030] According to the present invention, the monovinyl aromatic hydrocarbon structural unit is a structural unit derived from monovinyl aromatic hydrocarbon, i.e., a structural unit formed by polymerization of monovinyl aromatic hydrocarbon. The monovinyl aromatic hydrocarbon may be any aromatic hydrocarbon monomer commonly used in the art with a vinyl substituent on the aromatic ring. Generally speaking, the monovinyl aromatic hydrocarbon has a structure shown in formula (1):

[0031]

[0032] Among them, R5 can be C6-C 20 The substituted or unsubstituted aryl group is preferably a phenyl group and a phenyl group substituted by one or more C1-C5 alkyl groups.

[0033] According to the present invention, the C6-C 20 Specific examples of substituted or unsubstituted aryl groups include, but are not limited to, phenyl, tolyl, ethylphenyl, tert-butylphenyl, dodecylphenyl, di-n-butylphenyl (including o-di-n-butylphenyl, m-di-n-butylphenyl and p-di-n-butylphenyl), n-propylphenyl and diethylphenyl (including o-di-n-ethylphenyl, m-di-n-ethylphenyl and p-di-n-ethylphenyl).

[0034] According to the present invention, the monovinyl aromatic hydrocarbon is selected from one or more of styrene, vinyl toluene, α-methylstyrene, 4-tert-butylstyrene and 4-methylstyrene.

[0035] According to the present invention, the conjugated diene structural unit is a structural unit derived from a conjugated diene, i.e., a structural unit formed by the polymerization of a conjugated diene. The conjugated diene refers to various unsaturated chain hydrocarbons containing a conjugated double bond (i.e., -C=CC=C-) in the molecular structure. The conjugated diene can be a conventional choice in the art, without particular limitation, and can be reasonably selected according to the application of the modified diene polymer finally obtained, for example, the conjugated diene can be selected from one or more of butadiene, isoprene, 1,3-pentadiene, 1,3-hexadiene and 2,3-dimethylbutadiene, preferably butadiene and / or isoprene.

[0036] In some embodiments of the present invention, the single-arm number average molecular weight of the modified diene polymer is 1,000-10,000 g / mol, and the molecular weight distribution is 1-1.3.

[0037] Preferably, the single-arm number average molecular weight of the modified diene polymer is 1,500-8,000 g / mol, and the molecular weight distribution is 1.05-1.2.

[0038] More preferably, the single-arm number average molecular weight of the modified diene polymer is 1,900-3,000 g / mol, and the molecular weight distribution is 1.07-1.1.

[0039] In the present invention, the single-arm number average molecular weight refers to the number average molecular weight of the diene polymer before coupling.

[0040] In the present invention, the single-arm number average molecular weight, molecular weight distribution and coupling efficiency can be measured by using an ALLIANCE 2690 gel permeation chromatograph (GPC) from WATERS, USA, with THF as the mobile phase, narrow distribution polystyrene as the standard sample, and the temperature being 25°C.

[0041] The second aspect of the present invention provides a method for preparing a modified diene polymer, the method comprising: in an inert atmosphere, in the presence of a first initiator, contacting a diene polymer containing a monovinyl aromatic hydrocarbon structural unit and a conjugated diene structural unit with a mercaptocarboxylic acid compound for reaction, wherein the contact conditions allow the mercaptocarboxylic acid compound to be chemically bonded to the diene polymer to form a mercaptocarboxylic acid side chain, thereby obtaining a modified diene polymer; based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chain is 1-10wt%; the general formula of the mercaptocarboxylic acid compound is HS-R-COOH, wherein R is selected from a linear or branched C1-C 10 Alkylene.

[0042] In some embodiments of the present invention, R is selected from a linear or branched C1-C 10 The alkylene group is preferably a methylene group or an ethylene group.

[0043] In some embodiments of the present invention, the mercaptocarboxylic acid compound is selected from mercaptoacetic acid and / or mercaptopropionic acid.

[0044] In some embodiments of the present invention, based on the total weight of the modified diene polymer, the content of the conjugated diene structural unit having a double bond in the side chain is 15-45 wt %, preferably 30-40 wt %.

[0045] According to the present invention, the inert atmosphere refers to any gas or gas mixture that does not chemically react with the reactants and products, such as nitrogen and one or more of the gases in Group 0 of the periodic table. The method for maintaining the inert atmosphere is to introduce any gas or gas mixture that does not chemically react with the reactants and products into the reaction system.

[0046] According to the present invention, the first initiator may be one or more free radical initiators such as azo initiators, peroxide initiators and redox initiators known to those skilled in the art.

[0047] The azo initiator can be selected from one or more of dimethyl azobisisobutyrate, azobisisobutyramidine hydrochloride, azodicarbonamide, azobisisopropylimidazoline hydrochloride, azoisobutylcyanoformamide, azobiscyclohexylcarbonitrile, azobiscyanovaleric acid, azobisisopropylimidazoline, azobisisobutyronitrile, azobisisovaleronitrile and azobisisoheptylonitrile.

[0048] The peroxide initiator may be selected from one or more of hydrogen peroxide, ammonium persulfate, sodium persulfate, potassium persulfate, benzoyl peroxide and tert-butyl benzoyl peroxide.

[0049] The redox initiator may be selected from one or more of sulfate-sulfite, persulfate-thiourea, persulfate-organic salt and ammonium persulfate-fatty amine. Specifically, the sulfate-sulfite may be selected from one or more of sodium sulfate-sodium sulfite, potassium sulfate-potassium sulfite and ammonium sulfate-ammonium sulfite; the persulfate-thiourea may be selected from one or more of sodium persulfate-thiourea, potassium persulfate-thiourea and ammonium persulfate-thiourea; the persulfate-organic salt may be selected from one or more of sodium persulfate-potassium acetate, potassium persulfate-potassium acetate and ammonium persulfate-ammonium acetate; the ammonium persulfate-fatty amine may be ammonium persulfate-N,N-tetramethylethylenediamine and / or ammonium persulfate-diethylamine.

[0050] In the present invention, based on the total weight of the modified diene polymer, the amount of the first initiator is 0.01-0.1 wt%, more preferably 0.01-0.08 wt%.

[0051] The present invention does not particularly limit the conditions for contacting the diene polymer with the mercaptocarboxylic acid compound, as long as it can chemically bond to the diene polymer. For example, the contact conditions generally include contact temperature, contact pressure and contact time. Generally speaking, in order to facilitate the chemical bonding of the mercaptocarboxylic acid compound to the diene polymer, the contact conditions include: contact temperature of 30-100°C, preferably 70-90°C; contact pressure of 0.01-1MPa, preferably 0.1-0.5MPa; contact time of 0.2-24h, preferably 0.5-5h.

[0052] In some embodiments of the present invention, the preparation method further comprises: after the reaction is completed, adding an antioxidant, and vacuum drying to obtain the modified diene polymer.

[0053] In the present invention, an antioxidant is added after the reaction is completed to further enhance the anti-aging performance of the rubber composition. In the present invention, the antioxidant is selected from one or more of antioxidant 1520, antioxidant 1076 and antioxidant 2246.

[0054] According to the present invention, after adding the antioxidant, the modified diene polymer can be precipitated from the solution by purification precipitation, centrifugal separation, filtration, decantation, rotary evaporation and the like, or the solvent in the reaction system can be removed by gas stripping, which is known to those skilled in the art and will not be described in detail herein. The antioxidant in the present invention does not participate in the grafting reaction and only exists in a mixed state.

[0055] According to the present invention, the vacuum drying conditions include: temperature of 50-70°C, preferably 60°C; time of 20-30h, preferably 24h; vacuum degree of 0.1MPa.

[0056] In some embodiments of the present invention, the method for preparing the diene polymer comprises: in an inert atmosphere, in the presence of a second initiator and optionally a structure regulator, first subjecting a monovinyl aromatic hydrocarbon to a first polymerization reaction in a solvent, then adding a conjugated diene to conduct a second polymerization reaction, and then adding a coupling agent to conduct a coupling reaction to obtain a diene polymer.

[0057] The purpose of initiating polymerization of monovinyl aromatic hydrocarbons first and then initiating polymerization of conjugated dienes in the present invention is to design and synthesize a soft-hard combined molecular structure. The purpose of adding a coupling agent after the reaction is to obtain suitable fluidity on the one hand and to reduce the free ends of the molecular chains on the other hand.

[0058] In some embodiments of the present invention, the coupling efficiency of the diene polymer is 50-95%, preferably 70-90%, and more preferably 80-90%.

[0059] In the present invention, the purpose of limiting the coupling efficiency of the diene polymer is to obtain suitable fluidity on the one hand, and to reduce the free ends of the molecular chains on the other hand.

[0060] In the present invention, since the modification process does not cause further coupling of the molecular chains, it can be considered that the coupling efficiency of the modified diene polymer is the same as that of the diene polymer.

[0061] In some embodiments of the present invention, the content of the monovinyl aromatic structural unit is 2-10 wt%, preferably 3-6 wt%; the content of the conjugated diene structural unit is 80-97 wt%, preferably 89-95 wt%;

[0062] In the present invention, the purpose of limiting the weight ratio of monovinyl aromatic hydrocarbon and conjugated diene hydrocarbon is to design a suitable molecular chain hardness length.

[0063] In some embodiments of the present invention, based on the total weight of the diene polymer, the content of the conjugated diene structural unit having a double bond in the side chain is 15-45 wt %, preferably 30-40 wt %.

[0064] In some embodiments of the present invention, based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chains is 2-5 wt %.

[0065] According to the present invention, in the preparation process of diene polymer, the second initiator can be various existing initiators capable of initiating the polymerization of conjugated diene, preferably, the second initiator is an organic lithium initiator. The organic lithium initiator can be, for example, a single organic lithium initiator with a molecular formula of RLi, wherein R is a linear or branched alkyl, cycloalkyl or aryl group. Specifically, the single organic lithium initiator is selected from one or more of ethyl lithium, propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, pentyl lithium, hexyl lithium, cyclohexyl lithium, phenyl lithium, methyl phenyl lithium and naphthyl lithium, more preferably, the initiator is n-butyl lithium and / or sec-butyl lithium. In addition, the present invention can also use a dilithium initiator, such as trimethylene dilithium and / or tetramethylene dilithium. The present invention has no particular restrictions on the amount of the second initiator, and can be reasonably selected according to the designed molecular weight. It should be easily understood by those skilled in the art that when it is necessary to prepare a diene polymer with a larger molecular weight, the amount of the second initiator can be reduced, but the polymerization rate will also be reduced accordingly; when it is necessary to prepare a diene polymer with a smaller molecular weight, the amount of the second initiator can be increased, but the polymerization rate will also be increased accordingly. Therefore, taking into account the polymerization rate and the molecular weight of the diene polymer obtained, preferably, the amount of the second initiator is 1.5-25mmol based on the total weight of 100g of conjugated diene I and conjugated diene II.

[0066] The present invention does not particularly limit the conditions of the second reaction, which generally include polymerization temperature, polymerization pressure and polymerization time. Among them, in order to be more conducive to the polymerization reaction, the polymerization temperature is preferably 0-80°C, more preferably 40-60°C; the polymerization pressure is preferably 0.05-0.5MPa, more preferably 0.1-0.3MPa. Generally speaking, the extension of the polymerization time is conducive to the improvement of the conversion rate of the reactants and the yield of the reaction products, but the increase in the conversion rate of the reactants and the yield of the reaction products is not obvious if the polymerization time is too long. Therefore, considering the polymerization efficiency and effect, the polymerization time is preferably 0.5-10h, more preferably 0.5-2h.

[0067] In some embodiments of the present invention, the conditions of the first polymerization reaction include: polymerization temperature of 0-80°C, preferably 40-60°C; polymerization pressure of 0.05-0.5MPa, preferably 0.1-0.3MPa; polymerization time of 0.5-5h, preferably 0.5-3h.

[0068] In some embodiments of the present invention, the conditions of the second polymerization reaction include: polymerization temperature of 0-80°C, preferably 40-60°C; polymerization pressure of 0.05-0.5MPa, preferably 0.1-0.3MPa; polymerization time of 0.5-5h, preferably 0.5-3h.

[0069] In the present invention, the pressure refers to the gauge pressure.

[0070] According to the present invention, in the process of preparing the diene polymer, the solvent can be any substance that can serve as a reaction medium. Preferably, the solvent is a hydrocarbon solvent and / or an ether solvent. The hydrocarbon solvent is one or more of C5-C7 cycloalkanes, aromatic hydrocarbons and isoalkanes. Specific examples of the hydrocarbon solvent include, but are not limited to, one or more of benzene, toluene, pentane, heptane, n-hexane and cyclohexane. The ether solvent is C4-C 15 Monoether and / or polyether. Specific examples of the ether solvent include, but are not limited to, tert-butoxyethoxyethane and / or tetrahydrofuran. These solvents can be used alone or in combination. The amount of the solvent can be reasonably selected according to the amount of the monomer. For example, the amount of the solvent can make the total concentration of the monovinyl aromatic hydrocarbon and the conjugated diene be 10-50wt%, preferably 20-40wt%.

[0071] According to the present invention, after the polymerization reaction is completed, a coupling agent can be added to the polymerization system to couple at least part of the diene polymers together. The type of the coupling agent is selected from one or more of polyvinyl compounds, halides, ethers, aldehydes, ketones, esters, etc. Preferably, the coupling agent is selected from one or more of divinylbenzene, dimethyldichlorosilane, tetravinylsilane, tetrachloromethane, silicon tetrachloride, tin tetrachloride, dimethyl terephthalate and epoxy soybean oil, more preferably, the coupling agent is selected from one or more of divinylbenzene, dimethyldichlorosilane, silicon tetrachloride, tin tetrachloride.

[0072] The present invention has no particular limitation on the amount of the coupling agent, which can be appropriately selected according to the amount of the initiator, with the coupling efficiency of the final product being 50-95%, preferably 70-90%, more preferably 80-90%.

[0073] According to the present invention, preferably, a structure regulator can also be added during the preparation process of the diene polymer, so that the microstructure of the diene polymer can be effectively controlled. The structure regulator can be various existing materials that can regulate the microstructure of the diene polymer, preferably, the structure regulator is selected from one or more of ether, dibutyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, diglyme, dioxane, crown ether, tetrahydrofurfuryl alcohol ether, triethylamine, tetramethylethylenediamine, hexamethylphosphoric triamide, potassium tert-butoxide, potassium tert-amyl alcohol, potassium lauryl alcohol, potassium alkylbenzene sulfonate and sodium alkylbenzene sulfonate. Generally speaking, the molar ratio of the structure regulator to the second initiator is 1-100:1, more preferably 80-100:1.

[0074] The third aspect of the present invention provides a modified diene polymer obtained by the aforementioned preparation method.

[0075] The fourth aspect of the present invention provides the use of the aforementioned modified diene polymer as a rubber processing aid in a rubber processing process.

[0076] The modified diene polymer of the present invention can be added into the rubber processing process as a rubber processing aid, which can improve the processability of the rubber and simultaneously meet the requirements of the rubber product for anti-slip property and low rolling resistance performance.

[0077] The fifth aspect of the present invention provides a rubber composition, which contains rubber and the aforementioned modified diene polymer; wherein the amount of the modified diene polymer is 5-30 parts by weight based on 100 parts by weight of the rubber composition.

[0078] In some embodiments of the present invention, the rubber is selected from one or more of natural rubber, polybutadiene rubber, styrene-butadiene rubber, polyisoprene rubber, chloroprene rubber, butyl rubber and ethylene-propylene-diene rubber.

[0079] A sixth aspect of the present invention provides a vulcanized rubber obtained by vulcanizing the rubber composition described above.

[0080] In the present invention, vulcanization can be carried out in a vulcanizing bed or a flat vulcanizing machine. The method and conditions for vulcanizing the rubber mix can be conventionally selected in the art. For example, the vulcanization reaction conditions include: the vulcanization temperature can be 140-180° C., the vulcanization pressure can be 10-15 MPa, and the vulcanization time can be 10-50 min.

[0081] A seventh aspect of the present invention provides use of the aforementioned rubber composition or the aforementioned vulcanized rubber in tire manufacturing or plastic modification, preferably in tire tread rubber.

[0082] The present invention is described in detail below by way of examples, but the protection scope of the present invention is not limited to the following description.

[0083] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0084] In the following preparation examples and comparative examples:

[0085] (1) The content of conjugated diene structural units with double bonds in the side chains, the content of monovinyl aromatic hydrocarbons, the content of conjugated diene, and the content of mercaptocarboxylic acid side chains in the polymer were all measured using an AVANCE DRX 400 MHz nuclear magnetic resonance spectrometer from Bruker, Switzerland, with deuterated chloroform as the solvent.

[0086] (2) The single-arm number average molecular weight, molecular weight distribution and coupling efficiency were measured using an ALLIANCE 2690 gel permeation chromatograph (GPC) from WATERS, USA, with THF as the mobile phase and narrow distribution polystyrene as the standard sample at a temperature of 25°C.

[0087] (3) The physical properties of the vulcanized rubber were measured using a Japanese SHIMADZU AG-20KNG tensile testing machine in accordance with GB / T528-1998.

[0088] (4) Vulcanization characteristics: Beijing Youshen C2000E rotorless vulcanizer, test temperature 160°C, oscillation rate 1.7 Hz, amplitude 1°.

[0089] Example 1

[0090] The examples are used to illustrate the modified diene polymer and the preparation method thereof provided by the present invention.

[0091] (1) In a 10L stainless steel stirred tank, under the protection of high-purity nitrogen, 4088g of cyclohexane, 10.1g of styrene and 1.0g of tetrahydrofuran were added, heated to 50°C, 0.55mol of n-butyl lithium was added, and the pressure was controlled at 0.2MPa, and the reaction was initiated for 0.5h, then 489.9g of butadiene was added, and after reacting for 1h, 0.06mol of tin tetrachloride was added, and the reaction was continued at 60°C for 0.5h to obtain a diene polymer with a coupling efficiency of 52%;

[0092] (2) Add 5.9 g of mercaptopropionic acid and 85 mg of azobisisobutyl cyanide to the diene polymer obtained in step (1), heat to 80° C., and control the pressure at 0.2 MPa. After reacting for 3 h, a reaction solution is obtained; add 0.2 g of antioxidant Irganox 1520 to the above reaction solution, and dry it in a vacuum at 60° C. for 24 h to obtain a modified diene polymer, which is labeled as Z1.

[0093] After testing, the single-arm number average molecular weight of the modified diene polymer is 1,200 g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 52%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 2wt%, the content of the butadiene structural unit is 96.84wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 1.16wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 18.9wt%.

[0094] Example 2

[0095] (1) In a 10L stainless steel stirred tank, under the protection of high-purity nitrogen, 4088g of cyclohexane, 15.6g of styrene and 0.3g of tetrahydrofurfuryl alcohol ether were added, heated to 50°C, 0.25mol of n-butyl lithium was added, and the pressure was controlled at 0.2MPa to initiate the reaction for 0.5h, then 484.4g of butadiene was added, and after reacting for 1h, 0.035mol of tin tetrachloride was added, and the reaction was continued at 60°C for 0.5h to obtain a diene polymer with a coupling efficiency of 61%;

[0096] (2) Add 11 g of mercaptopropionic acid and 85 mg of azobisisobutyl cyanide to the diene polymer obtained in step (1), heat to 80° C., and control the pressure at 0.2 MPa. After reacting for 3 h, a reaction solution is obtained; add 0.2 g of antioxidant Irganox 1520 to the above reaction solution, and dry it in a vacuum at 60° C. for 24 h to obtain a modified diene polymer, which is labeled as Z2.

[0097] After testing, the single-arm number average molecular weight of the modified diene polymer is 1,900 g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 61%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 3.05wt%, the content of the butadiene structural unit is 94.75wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 2.2wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 25.8wt%.

[0098] Example 3

[0099] (1) In a 10L stainless steel stirred tank, under the protection of high-purity nitrogen, 4088g of cyclohexane, 24.5g of styrene and 0.8g of tetrahydrofurfuryl alcohol ether were added, heated to 50°C, 0.25mol of n-butyl lithium was added, and the pressure was controlled at 0.2MPa to initiate the reaction for 0.5h, then 475.5g of butadiene was added, and after reacting for 1h, 0.05mol of tin tetrachloride was added, and the reaction was continued at 60°C for 0.5h to obtain a diene polymer with a coupling efficiency of 72%;

[0100] (2) Add 15 g of mercaptopropionic acid and 90 mg of azobisisobutyl cyanide to the diene polymer obtained in step (1), heat to 80° C., and control the pressure at 0.2 MPa. After reacting for 3 h, a reaction solution is obtained; add 0.3 g of antioxidant Irganox 1520 to the above reaction solution, and dry it in a vacuum at 60° C. for 24 h to obtain a modified diene polymer, which is marked as Z3.

[0101] After testing, the single-arm number average molecular weight of the modified diene polymer is 1,900 g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 72%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 4.75wt%, the content of the butadiene structural unit is 92.35wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 2.9wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 31.7wt%.

[0102] Example 4

[0103] (1) In a 10L stainless steel stirred tank, under the protection of high-purity nitrogen, 4088g of cyclohexane, 30.5g of styrene and 1.3g of tetrahydrofurfuryl alcohol ether were added, heated to 50°C, 0.20mol of n-butyl lithium was added, and the pressure was controlled at 0.2MPa to initiate the reaction for 0.5h, then 469.5g of butadiene was added, and after reacting for 1h, 0.06mol of tin tetrachloride was added, and the reaction was continued at 60°C for 0.5h to obtain a diene polymer with a coupling efficiency of 82%;

[0104] (2) Add 22 g of mercaptopropionic acid and 90 mg of azobisisobutyl cyanide to the diene polymer obtained in step (1), heat to 80° C., and control the pressure at 0.2 MPa. After reacting for 3 h, a reaction solution is obtained; add 0.3 g of antioxidant Irganox 1520 to the above reaction solution, and dry it in a vacuum at 60° C. for 24 h to obtain a modified diene polymer, which is marked as Z4.

[0105] After testing, the single-arm number average molecular weight of the modified diene polymer is 2,500 g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 82%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 5.84wt%, the content of the butadiene structural unit is 89.96wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 4.2wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 36.5wt%.

[0106] Example 5

[0107] (1) In a 10L stainless steel stirred tank, under the protection of high-purity nitrogen, 4088g of cyclohexane, 38.5g of styrene and 1.8g of tetrahydrofurfuryl alcohol ether were added, heated to 40°C, 0.11mol of n-butyl lithium was added, and the pressure was controlled at 0.2MPa to initiate the reaction for 0.5h, then 461.5g of butadiene was added, and after reacting for 1h, 0.04mol of tin tetrachloride was added, and the reaction was continued at 60°C for 0.5h to obtain a diene polymer with a coupling efficiency of 88%;

[0108] (2) Add 35 g of mercaptopropionic acid and 90 mg of azobisisobutyl cyanide to the diene polymer obtained in step (1), heat to 80° C., and control the pressure at 0.2 MPa. After reacting for 3 h, a reaction solution is obtained; add 0.3 g of antioxidant Irganox 1520 to the above reaction solution, and dry it in a vacuum at 60° C. for 24 h to obtain a modified diene polymer, which is marked as Z5.

[0109] After testing, the single-arm number average molecular weight of the modified diene polymer is 4,800 g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 88%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 7.19wt%, the content of the butadiene structural unit is 86.31wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 6.5wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 42.5wt%.

[0110] Example 6

[0111] The same preparation method as in Example 5 was used, except that the mercaptopropionic acid was replaced by an equal amount of mercaptoacetic acid, and other conditions remained unchanged, to obtain a modified diene polymer, which was labeled as Z6.

[0112] After testing, the single-arm number average molecular weight of the modified diene polymer is 4,800 g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 88%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 7.19wt%, the content of the butadiene structural unit is 86.31wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 6.5wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 41.6wt%.

[0113] Example 7

[0114] The same preparation method as in Example 5 was used, except that the mercaptopropionic acid was replaced by 40 g of thioglycolic acid, and other conditions remained unchanged, to obtain a modified diene polymer, which was labeled as Z7.

[0115] After testing, the single-arm number average molecular weight of the modified diene polymer is 0.48 thousand g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 88%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 7.13wt%, the content of the butadiene structural unit is 85.47wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 7.4wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 40.3wt%.

[0116] Example 8

[0117] The same preparation method as in Example 5 was used, except that the mercaptopropionic acid was replaced by 50 g of mercaptoacetic acid, and other conditions remained unchanged, to obtain a modified diene polymer, which was labeled as Z8.

[0118] After testing, the single-arm number average molecular weight of the modified diene polymer is 0.48 thousand g / mol, and the molecular weight distribution is 1.1; the coupling efficiency is 88%; based on the total weight of the modified diene polymer, the content of the styrene structural unit is 7.0wt%, the content of the butadiene structural unit is 83.9wt%, the content of the mercaptocarboxylic acid structural unit hanging on the side chain is 9.1wt%, of which the content of the conjugated diene structural unit containing a double bond in the side chain is 39.3wt%.

[0119] Comparative Example 1

[0120] According to the same preparation method as in Example 5, except that only step (1) is included, a diene polymer with a coupling efficiency of 88% is obtained, which is marked as D1.

[0121] Application Example 1

[0122] The application examples are used to illustrate the vulcanized rubber and the preparation method thereof provided by the present invention.

[0123] (1) Preparation of rubber compound:

[0124] Vulcanized basic formula:

[0125] Olefin rubber SSBR2305 (styrene content 25wt%, vinyl content 30wt%): 100g; modified diene polymer Z1 prepared in Example 1: 15g; reinforcing agent carbon black: 55g; vulcanizing agent sulfur: 1g; vulcanization accelerator TBBS: 1g; activator stearic acid: 2g; antioxidant 4010: 1g; activator zinc oxide: 5g.

[0126] The mixture was kneaded on an open mixing mill at 50±5°C for 30 minutes to obtain a rubber compound H1.

[0127] (2) Vulcanization:

[0128] The mixed rubber H1 obtained in step (1) was vulcanized on a flat vulcanizer at 145° C. and 10 MPa for 35 minutes to obtain a vulcanized rubber S1.

[0129] Application Example 2-7

[0130] Application Examples 2-7 are used to illustrate the vulcanized rubber and the preparation method thereof provided by the present invention.

[0131] Vulcanized rubber was prepared in the same manner as in Application Example 1, except that the "modified diene polymer Z1 prepared in Example 1" in Application Example 1 was replaced by "modified diene polymers Z2-Z8 prepared in Examples 2-8", respectively; and the components in the rubber composition and their contents were specifically shown in Table 1; the rubber compounds H2-H8 were mixed at 50±5°C on an open mixing mill for 30 minutes to obtain rubber compounds H2-H8, and the obtained rubber compounds H2-H8 were vulcanized on a flat vulcanizer at 145°C and 10 MPa for 35 minutes to obtain vulcanized rubbers S2-S8.

[0132] Comparative application example 1

[0133] A vulcanized rubber was prepared in the same manner as in Application Example 5, except that the "modified diene polymer Z5 prepared in Example 5" in Application Example 5 was replaced by the "diene polymer D1 prepared in Comparative Example 1"; and the components in the rubber composition and their contents were specifically shown in Table 1; the rubber mix was mixed on an open mixing mill at 50±5°C for 30 min to obtain a rubber mix HD1, and the obtained rubber mix HD1 was vulcanized on a flat vulcanizer at 145°C and 10 MPa for 35 min to obtain a vulcanized rubber SD1.

[0134] Comparative Application Example 2

[0135] The vulcanized rubber was prepared in the same manner as in Application Example 5, except that the modified diene polymer Z5 prepared in Example 5 was replaced by aromatic oil, and the other conditions were the same, to obtain the vulcanized rubber SD2.

[0136] Table 1 Components and their contents

[0137]

[0138]

[0139] Test Example 1-8

[0140] Test Examples 1-8 are used to illustrate the performance tests of the vulcanized rubbers S1-S8 provided by the present invention.

[0141] (1) Glass transition temperature (Tg) test:

[0142] The measurement was performed using a differential scanning calorimetry (DSC) instrument of TA Corporation, USA, model MDSC2910, wherein the modulation period was 60 s, the modulation amplitude was ±1.5°C, the heating rate was 10°C / min, nitrogen protection was used, and the flow rate was 50 mL / min. The results are shown in Table 1.

[0143] (2) Mechanical properties test:

[0144] The vulcanized rubbers S1-S8 obtained in Application Examples 1-8 were respectively made into 2 mm thick vulcanized rubber sheets, and the obtained vulcanized rubber sheets were cut into dumbbell-shaped standard sheets according to the Type 1 dumbbell-shaped cutter specified in GB / T528-1998. The mechanical properties of the vulcanized rubber sheets were tested using a rubber tensile machine (produced by Shimadzu Corporation of Japan, model AG-20KNG), wherein the test temperature was 25°C and the pulling speed was 500 mm / min. The breaking strength and breaking elongation of the vulcanized rubber were obtained, and the results are shown in Table 1.

[0145] (3) Shore A hardness test:

[0146] The test was carried out according to the method specified in GB / T531-1999, and the results are shown in Table 1;

[0147] (4) Anti-deformation performance test:

[0148] Cut the vulcanized rubber S1-S8 into dumbbell-shaped standard pieces according to the type 1 dumbbell-shaped cutter specified in GB / T528-92, and break the sample at a test temperature of 25°C and a pulling speed of 500 mm / min. Place the sample after tensile fracture for 3 minutes, then fit the two broken parts together, measure the distance between the two parallel lines after fitting, and calculate the tearing permanent deformation value according to the following formula:

[0149] S b =100(L t -L0) / L0, where S b is the permanent deformation at break, %; L t is the distance between the two parallel lines after the specimens are matched, mm; L0 is the initial test length, mm. The results are shown in Table 1.

[0150] (5) Heat generation performance test:

[0151] The test was conducted using a Y3000E compression heat tester from Beijing Youshen Electronic Instrument Co., Ltd., where the test temperature was 55°C, the test time was 25 minutes, and the compression frequency was 30 times / second. The results are shown in Table 1.

[0152] (6) Tests of anti-skid performance and rolling resistance:

[0153] The anti-wet skid performance and rolling resistance of vulcanized rubber S1-S8 were measured using the DMA-2980 viscoelastic spectrometer of TA Company in the United States. The test frequency was 2Hz, the heating rate was 5℃ / min, the test temperature was 100℃, and the sample size was 40mm×5mm×1mm. Tanδ at 0℃ is used to represent the anti-wet skid performance of vulcanized rubber. The larger the tanδ, the better the anti-wet skid performance of the vulcanized rubber; tanδ at 60℃ is used to represent the rolling resistance of the vulcanized rubber. The smaller the tanδ, the smaller the rolling resistance of the vulcanized rubber; the dispersion of fillers in rubber is characterized by the value of Tanδ(0℃) / Tanδ(60℃). The higher the value, the better the dispersion of fillers. The results are shown in Table 2.

[0154] Comparative test example 1-2

[0155] The properties of the reference vulcanized rubbers SD1-SD2 obtained from comparative application examples 1-2 were tested according to the methods of test examples 1-8, and the results are shown in Table 2.

[0156] Table 2 Physical properties data

[0157]

[0158]

[0159] Table 2 Physical properties data table (continued)

[0160]

[0161] Note: It should be noted that in Table 2, Mooney relaxation t 70 / s is the time it takes for Mooney to drop by 70%; t 80 / s is the time it takes for Mooney to drop by 80%; t 90 / s is the time for Mooney to drop by 90%; intercept K is the Mooney value at the moment of Mooney relaxation of 1 second, which can reflect the initial shrinkage of the material; slope a is the slope of the Mooney stress relaxation line, which reflects the speed of stress relaxation; area A is the area under the relaxation line, which is a comprehensive reflection of the performance of Mooney relaxation; Tanδ(0℃) / Tanδ(60℃) ratio reflects the dispersion of filler in rubber, and the larger the ratio, the better the dispersion effect.

[0162] From the results in Table 2, we can see that:

[0163] (1) The modified diene polymers Z1-Z8 prepared in Examples 1-8 of the present invention can be added to the rubber mixing process to obtain good processability, that is, good agglomeration. Compared with the comparative example 1 using environmentally friendly aromatic oil, the modified diene polymers Z1-Z8 have better processability, which is manifested in having a lower Mooney relaxation area A during the rubber mixing process.

[0164] (2) The ratio of Tanδ(0℃) / Tanδ(60℃) reflects the dispersion of the filler in the rubber. The larger the ratio, the better the dispersion effect. It can be seen that both Examples 1-8 of the present invention and Comparative Example 1 can promote the dispersion of the filler very well. However, Examples 1-8 are more conducive to improving the anti-slip property of the rubber, that is, the Tan(0℃) values ​​of Examples 1-8 are all higher than that of Comparative Example 1, which is conducive to improving the anti-slip property of the rubber (for example, shoe material); at the same time, the Tan(60℃) values ​​of Examples 1-8 are all lower than that of Comparative Example 1, which reduces the rolling resistance and improves its comprehensive dynamic performance.

[0165] (3) The hardness, tear strength, permanent deformation, elongation and 300% modulus of Examples 1-8 are basically the same as those of Comparative Example 1, and only the tear strength is slightly improved. Therefore, the method of the present invention will not have a significant effect on these physical and mechanical properties.

[0166] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A modified diene polymer, characterized in that: The modified diene polymer comprises a main chain containing monovinyl aromatic structural units and conjugated diene structural units and a mercaptocarboxylic acid side chain suspended from the main chain, wherein the content of the mercaptocarboxylic acid side chain is 1-10wt% based on the total weight of the modified diene polymer; the general formula of the mercaptocarboxylic acid side chain is -SR-COOH, wherein R is selected from a linear or branched C1-C 10 Alkylene.

2. The modified diene polymer according to claim 1, wherein R is selected from a linear or branched C1-C 10 The alkylene group is preferably a methylene group or an ethylene group.

3. The modified diene polymer according to claim 1 or 2, wherein Based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chain is 2-5wt%.

4. The modified diene polymer according to any one of claims 1 to 3, wherein Based on the total weight of the modified diene polymer, the content of the conjugated diene structural unit having a double bond in the side chain is 15-45wt%, preferably 30-40wt%; Preferably, the coupling efficiency of the modified diene polymer is 50-95%, preferably 70-90%, more preferably 80-90%.

5. The modified diene polymer according to any one of claims 1 to 4, wherein Based on the total weight of the modified diene polymer, the content of the monovinyl aromatic structural unit is 2-10wt%, preferably 3-6wt%; the content of the conjugated diene structural unit is 80-97wt%, preferably 89-95wt%; Preferably, the monovinyl aromatic hydrocarbon structural unit is a structural unit derived from monovinyl aromatic hydrocarbon; the monovinyl aromatic hydrocarbon has a structure shown in formula (1): Wherein R5 is selected from C6-C 20 The substituted or unsubstituted aryl group is preferably a phenyl group and a phenyl group substituted by one or more C1-C5 alkyl groups; preferably, the monovinyl aromatic hydrocarbon is selected from one or more of styrene, vinyl toluene, α-methylstyrene, 4-tert-butylstyrene and 4-methylstyrene; Preferably, the conjugated diene structural unit is a structural unit derived from a conjugated diene; preferably, the conjugated diene is selected from one or more of butadiene, isoprene, 1,3-pentadiene, 1,3-hexadiene and 2,3-dimethylbutadiene, more preferably butadiene and / or isoprene.

6. The modified diene polymer according to any one of claims 1 to 5, wherein The single-arm number average molecular weight of the modified diene polymer is 10,000-10,000 g / mol, and the molecular weight distribution is 1-1.3; Preferably, the single-arm number average molecular weight of the modified diene polymer is 1,500-8,000 g / mol, and the molecular weight distribution is 1.05-1.2; More preferably, the single-arm number average molecular weight of the modified diene polymer is 1,900-3,000 g / mol, and the molecular weight distribution is 1.07-1.

1.

7. A method for preparing a modified diene polymer, characterized in that: The preparation method comprises: in an inert atmosphere, in the presence of a first initiator, contacting a diene polymer containing a monovinyl aromatic hydrocarbon structural unit and a conjugated diene structural unit with a mercaptocarboxylic acid compound for reaction, wherein the contact conditions allow the mercaptocarboxylic acid compound to be chemically bonded to the diene polymer to form a mercaptocarboxylic acid side chain, thereby obtaining a modified diene polymer; based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chain is 1-10 wt %; the general formula of the mercaptocarboxylic acid compound is HS-R-COOH, wherein R is selected from a linear or branched C1-C 10 Alkylene.

8. The preparation method according to claim 7, wherein: R is selected from a linear or branched C1-C 10 Alkylene is preferably methylene or ethylene; preferably, the mercaptocarboxylic acid compound is selected from mercaptoacetic acid and / or mercaptopropionic acid; and / or, based on the total weight of the modified diene polymer, the content of the conjugated diene structural unit having a double bond in the side chain is 15-45wt%, preferably 30-40wt%; And / or, based on the total weight of the modified diene polymer, the content of the mercaptocarboxylic acid side chains is 2-5 wt%.

9. The preparation method according to claim 7 or 8, wherein: The first initiator is selected from one or more of an azo initiator, a peroxide initiator and a redox initiator; preferably, based on the total weight of the modified diene polymer, the amount of the first initiator is 0.01-0.1wt%, more preferably 0.01-0.08wt%; And / or, the contact conditions include: contact temperature of 30-100°C, preferably 70-90°C; contact pressure of 0.01-1MPa, preferably 0.1-0.5MPa; contact time of 0.2-24h, preferably 0.5-5h; And / or, the preparation method further comprises: after the reaction is completed, adding an antioxidant, and vacuum drying to obtain the modified diene polymer; preferably, the antioxidant is selected from one or more of antioxidant 1520, antioxidant 1076 and antioxidant 2246.

10. The preparation method according to any one of claims 7 to 9, wherein: The method for preparing the diene polymer comprises: in an inert atmosphere, in the presence of a second initiator and optionally a structure regulator, firstly subjecting monovinyl aromatic hydrocarbon to a first polymerization reaction in a solvent, then adding a conjugated diene to a second polymerization reaction, and then adding a coupling agent to conduct a coupling reaction to obtain the diene polymer; Preferably, the coupling efficiency of the diene polymer is 50-95%, preferably 70-90%, more preferably 80-90%; Preferably, based on the total weight of the modified diene polymer, the content of the monovinyl aromatic structural unit is 2-10 wt%, preferably 3-6 wt%; the content of the conjugated diene structural unit is 80-97 wt%, preferably 89-95 wt%.

11. The preparation method according to claim 10, wherein: The second initiator is an organic lithium initiator selected from one or more of ethyl lithium, propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, pentyl lithium, hexyl lithium, cyclohexyl lithium, phenyl lithium, methylphenyl lithium, naphthyl lithium, trimethylene dilithium and tetramethylene dilithium; preferably, the amount of the second initiator is 1.5-25 mmol based on the total weight of 100 g of conjugated diene I and conjugated diene II; And / or, the structure regulator is selected from one or more of ether, dibutyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dioxane, crown ether, tetrahydrofurfuryl alcohol ether, triethylamine, tetramethylethylenediamine, hexamethylphosphoric triamide, potassium tert-butoxide, potassium tert-amyl alcohol, potassium lauryl alcohol, potassium alkylbenzene sulfonate and sodium alkylbenzene sulfonate; preferably, the molar ratio of the structure regulator to the second initiator is 1-100:1, more preferably 80-100:1; And / or, the solvent is selected from hydrocarbon solvents and / or ether solvents; preferably, the hydrocarbon solvent is selected from one or more of benzene, toluene, pentane, heptane, n-hexane and cyclohexane; the ether solvent is selected from tert-butoxyethoxyethane and / or tetrahydrofuran; And / or, the coupling agent is selected from one or more of polyvinyl compounds, halides, ethers, aldehydes, ketones and esters; preferably, the coupling agent is selected from one or more of divinylbenzene, dimethyldichlorosilane, tetravinylsilane, tetrachloromethane, silicon tetrachloride, tin tetrachloride, dimethyl terephthalate and epoxy soybean oil; more preferably, the coupling agent is selected from one or more of divinylbenzene, dimethyldichlorosilane, silicon tetrachloride and tin tetrachloride; And / or, the conditions of the first polymerization reaction include: polymerization temperature of 0-80°C, preferably 40-60°C; polymerization pressure of 0.05-0.5MPa, preferably 0.1-0.3MPa; polymerization time of 0.5-5h, preferably 0.5-3h; And / or, the conditions of the second polymerization reaction include: polymerization temperature of 0-80°C, preferably 40-60°C; polymerization pressure of 0.05-0.5MPa, preferably 0.1-0.3MPa; polymerization time of 0.5-5h, preferably 0.5-3h.

12. The modified diene polymer obtained by the preparation method according to any one of claims 7 to 11.

13. Use of the modified diene polymer according to any one of claims 1 to 6 and 12 as a rubber processing aid in a rubber processing process.

14. A rubber composition, characterized in that: The rubber composition contains rubber and the modified diene polymer according to any one of claims 1 to 6 and 12; wherein the amount of the modified diene polymer is 5 to 30 parts by weight based on 100 parts by weight of the rubber composition.

15. The rubber composition according to claim 14, wherein The rubber is selected from one or more of natural rubber, polybutadiene rubber, styrene-butadiene rubber, polyisoprene rubber, chloroprene rubber, butyl rubber and EPDM rubber.

16. A vulcanized rubber, characterized in that: The vulcanized rubber is obtained by vulcanizing the rubber composition according to claim 14 or 15; Preferably, the vulcanization conditions include: vulcanization temperature of 140-180° C., vulcanization pressure of 10-15 MPa, and vulcanization time of 10-50 min.

17. Use of the rubber composition according to any one of claims 14 to 15 or the vulcanized rubber according to claim 16 in tire manufacturing or plastic modification, preferably in tire tread rubber.

Citation Information

Patent Citations

  • Modified conjugated diene polymer, preparation method thereof and styrene butadiene rubber

    CN107586362A

  • Rubber composition and vulcanized rubber

    CN115785545A

Cited By

  • Long-chain branching modification method of rare earth isoprene rubber and / or butadiene-isoprene rubber

    CN122103413A