Water-based fluorine-containing hybrid acrylic resin dispersion and preparation method thereof
By grafting the epoxy structure on the acrylic resin molecular chain and introducing monomers such as fluorine-containing and unsaturated fatty acids, aqueous fluorine-containing hybrid acrylic resin dispersions, the water resistance of traditional aqueous acrylic resin coatings on electronic equipment is solved. The problem of insufficient solvent resistance and adhesion has achieved the improvement of the comprehensive performance of the coating film and the feasibility of industrial production.
Patent Information
- Application Number
- CN202411351465.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional water-based acrylic resin coatings have insufficient water resistance, solvent resistance and adhesion on precision devices such as electronic equipment, and require external emulsifiers to be stable dispersed, affecting the comprehensive performance of the coating film.
By grafting epoxy structural units on the acrylic resin molecular chain and introducing fluorine-containing monomers, unsaturated fatty acids and hydrophilic monomers, free radical copolymerization process is used to prepare aqueous fluorine-containing hybrid acrylic resin dispersions to improve the coating film Adhesion, salt spray resistance and self-cleaning ability to avoid the use of added emulsifiers.
It significantly improves the mechanical properties, water resistance, solvent resistance, low temperature brittleness, high temperature retardation and self-cleaning ability of the coating film, solves the adhesion and weather resistance of traditional water-based acrylic resin coatings on electronic equipment, and saves energy in the process Environmentally friendly, suitable for industrial production.
Smart Images

Figure CN119060274A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer material synthesis, and particularly relates to an aqueous fluorine-containing hybrid acrylic resin dispersion and a preparation method thereof. Background Art
[0002] Waterborne acrylic resin coatings are widely used in industrial coatings, home decoration, rail transit and other fields due to their excellent weather resistance, chemical stability, colorability, moderate price and construction performance. However, since waterborne acrylic resins need to introduce a large number of hydrophilic groups or use a large amount of emulsifiers on acrylic resins, the water resistance, salt spray resistance and self-cleaning ability of the final coating are seriously affected. In addition, traditional acrylic resins are mostly linear structures, and resin film formation is difficult to form a three-dimensional network structure due to the lack of active functional groups. Therefore, the comprehensiveness of waterborne acrylic resin coatings needs to be improved.
[0003] At present, scholars have many methods to modify acrylic resin, such as epoxy resin grafting modification, silicone modification, inorganic nanoparticle resistance, functional monomer copolymerization modification, etc. However, a single modification method can only significantly improve a single performance, and it is difficult to achieve the purpose of improving the comprehensive performance of water-based acrylic resin. Electronic equipment is an important communication tool in our daily life, and its service life is long, which makes the coatings for protecting and decorating electronic equipment and its electronic devices, optoelectronic materials, nanocomposites, etc. have high requirements. For example, the coatings must have good RCA resistance, alcohol resistance, high hardness, and water boiling resistance. Water-based coatings have the advantages of low VOC and convenient construction and application, and are favored by the market. Therefore, it is urgent to develop water-based acrylic resins and their preparation processes with good comprehensive performance, moderate cost, and easy industrial production to meet the application of water-based acrylic coatings in electronic devices, optoelectronic materials, nanocomposites, industrial corrosion protection and other fields.
[0004] Patent CN 115873184 A discloses an epoxy resin modified waterborne acrylic resin dispersion, which adopts a semi-continuous seed free radical polymerization process and uses epoxy resin and other modified acrylic resins to prepare a waterborne acrylic resin dispersion and its downstream product, a waterborne acrylic industrial coating, which has the characteristics of good optical properties, fast drying speed, excellent water resistance and salt spray resistance, high hardness, etc. The product is green and environmentally friendly, with moderate cost, in line with the development trend of the industry, and has broad application prospects in the fields of electronic devices, optoelectronic materials, nanocomposites, etc. However, the coating of precision devices such as electronic equipment has the problem of poor water resistance and solvent resistance.
[0005] Patent CN 116120501 A discloses a silicone-fluorine / alkyd resin modified water-based acrylic resin dispersion and its preparation method, which is used to solve the problems of low solid and high viscosity of water-based acrylic resin dispersion, poor gloss retention after film formation, poor water resistance and low alkali resistance; the fluorinated polyether acrylic acid used improves the water resistance of acrylic resin, the alkyd resin is used to balance the film hardness of the resin dispersion, and the hydrophilic group of the alkyd resin can improve the hydrophilicity, so that the modified acrylic resin can be dispersed in water without emulsifiers, and the influence of emulsifiers on the mechanical properties, water resistance and gloss of the coating is avoided. The water resistance and stability of the dispersion after film coating are improved. However, due to the molecular structure characteristics of the alkyd resin itself, it has defects in weather resistance, so the weather resistance of the modified resin coating needs to be improved, and the patent does not involve adhesion. Summary of the invention
[0006] In view of the above technical problems, the present invention proposes an aqueous fluorinated hybrid acrylic resin dispersion and a preparation method thereof, which improves the adhesion and salt spray resistance of the acrylic resin by grafting epoxy structural units on the acrylic resin molecular chain, thereby solving the problem that traditional acrylic coatings have poor adhesion to metal substrates and insufficient salt spray resistance.
[0007] The technical solution for realizing the present invention is: 132-180 parts of epoxy resin, 39-57 parts of hydrophilic monomer, 62-94 parts of unsaturated fatty acid, 18-31 parts of glycidyl methacrylate, 30-100 parts of vinyl fluoride monomer, 110-180 parts of vinyl soft monomer, 130-200 parts of vinyl hard monomer, 1-3 parts of tertiary amine catalyst, 223-396 parts of solvent, 10-27 parts of initiator, 25-45 parts of neutralizer and 744-908 parts of deionized water.
[0008] The preparation method of the aqueous fluorinated hybrid acrylic resin dispersion comprises the following steps: (1) Weigh the epoxy resin according to the formula and place it in a reactor at 130℃-150℃, and replace the air in the reactor with N2. After the temperature stabilizes, add the hydrophilic monomer and tertiary amine catalyst and react at a constant temperature for 2-3 hours; (2) slowly adding unsaturated fatty acid and glycidyl methacrylate to (1), controlling the addition time to be 20-30 min, and then continuing the reaction for 2-3 h to obtain a vinyl epoxy resin prepolymer; (3) Weighing vinyl fluoride monomer, vinyl soft monomer, vinyl hard monomer and initiator according to the formula, and mixing them uniformly by ultrasonication to obtain a monomer mixture; (4) Cooling the epoxy resin prepolymer obtained in step (2) to 55-75°C, adding a co-solvent and stirring at a constant temperature for 20-30 minutes until the mixture is uniformly mixed; then heating to 85-95°C, dripping the monomer mixture in step (3), controlling the total dripping time to be 3.5-5.5 hours, and keeping the temperature for 3-5 hours after the dripping is completed to obtain a water-based fluorinated hybrid acrylic resin; (5) Cooling the aqueous fluorinated hybrid acrylic resin obtained in step (4) to 60-70° C., adding a neutralizing agent, adjusting the pH of the system to between 7.5 and 8.5, rapidly stirring for 30-35 min, then slowly adding deionized water for high-speed dispersion for 1-1.5 h, filtering, and obtaining an aqueous fluorinated hybrid acrylic resin dispersion with a solid content of 35-40% and a particle size of 160-190 nm.
[0009] The epoxy value of the epoxy resin used to prepare the aqueous fluorine-containing hybrid acrylic resin dispersion is 0.35-0.55 mol / 100g, preferably E-51 epoxy resin or BE188EL epoxy resin; the E-51 epoxy resin is preferably Sanmu brand E-51 epoxy resin; the unsaturated fatty acid is linoleic acid.
[0010] The hydrophilic monomer for preparing the aqueous fluorine-containing hybrid acrylic resin dispersion is one or a combination of 2,2-dihydroxymethylpropionic acid and 2-2-dihydroxymethylbutanoic acid.
[0011] The vinyl fluorine monomer for preparing the aqueous fluorine-containing hybrid acrylic resin dispersion is vinyloxyethyl perfluorooctanoate, and its structural formula is: .
[0012] The vinyl soft monomer for preparing the aqueous fluorine-containing hybrid acrylic resin dispersion is selected from one or any combination of butyl methacrylate, butyl acrylate, n-octyl acrylate, lauryl acrylate, isooctyl acrylate, vinyl acetate, isooctyl methacrylate, and n-octyl methacrylate; the vinyl hard monomer is selected from one or any combination of methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, benzyl acrylate, phenyl acrylate, styrene, divinyl benzene, and acrylonitrile.
[0013] The catalyst for preparing the aqueous fluorine-containing hybrid acrylic resin dispersion is tetrabutylammonium bromide; the initiator is one or a combination of azobisisobutyronitrile and azobisisoheptanenitrile; and the solvent is one or a combination of propylene glycol methyl ether and propylene glycol monobutyl ether.
[0014] The neutralizing agent for preparing the aqueous fluorine-containing hybrid acrylic resin dispersion is at least one of triethylamine and N,N-dimethylethanolamine.
[0015] The present invention introduces dimethylol propionic acid or dimethylol butyric acid with strong hydrophilicity through polycondensation when preparing epoxy resin prepolymer, so as to achieve water dispersibility of resin, solve the problem that traditional water-based acrylic paint needs to add emulsifier to achieve stable dispersion, and improve the storage stability of resin dispersion and downstream coating products; by introducing long-chain fatty acid structure, the prepared resin contains a certain number of double bonds, and the oxidative cross-linking of resin can be achieved in the film-forming process, so as to improve the problems of hot viscosity and cold brittleness, poor water resistance and salt spray resistance of resin; by introducing fluorine-containing monomer, the surface tension and surface energy are reduced, and the self-cleaning ability of resin is improved. Finally, the comprehensive properties of the coating, such as mechanical properties, water resistance, solvent resistance, low-temperature brittleness, high-temperature re-adhesion, self-cleaning, etc., are improved at the same time.
[0016] The beneficial effects of the present invention are: The present invention introduces a fluorine-containing monomer with strong hydrophobicity into acrylic resin through free radical copolymerization, thereby reducing the surface energy of the resin coating and improving the self-cleaning ability of the resin and the subsequent paint film; the introduction of unsaturated fatty acids ensures that the prepared resin contains unsaturated double bonds, which can be oxidatively cross-linked during the resin film-forming process, thereby improving the water resistance, salt spray resistance, acid and alkali resistance and hardness of the resin. At the same time, the double bond oxidative cross-linking process introduced by the unsaturated fatty acids will bind the fluorine elements that migrate to the coating surface and fix them on the coating surface, thereby avoiding the migration of fluorine elements to the inside of the coating caused by external factors such as immersion in water, acid and alkali immersion, contact with organic solvents, etc., and ensuring the permanence of the fluorine elements on the surface of the resin coating. By introducing active double bonds at the end of the epoxy resin molecular chain, the copolymerization ability with acrylic monomers is improved, and the problem of low grafting rate of epoxy resin on acrylic resin molecular chain is solved; by introducing dimethylol propionic acid or dimethylol butyric acid to modify the epoxy resin, a hydrophilic structural unit is introduced into the epoxy resin molecular chain, so that the finally prepared epoxy resin modified acrylic resin has a certain hydrophilicity, and can achieve self-emulsification without the addition of an emulsifier, solving the problems of water resistance, salt spray resistance and poor adhesion caused by emulsification of traditional water-based acrylic resins. The introduction of hydroxyl monomers in the resin preparation process improves the wetting and dispersibility of the resin and the pigment and filler, and improves the storage stability of the final coating product. This modification method is not only energy-saving and environmentally friendly, but also has moderate cost. The equipment for producing the resin is relatively simple, easy to industrialize, and has a good application market. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1This is the infrared curve of the dispersion coating prepared in Example 1 of the present invention.
[0019] Figure 2 This is the thermal gravimetric test curve of the dispersion coating film prepared in Example 1.
[0020] Figure 3 This is the DSC test graph of the dispersion coating film prepared in Example 1.
[0021] Figure 4 The particle size test results of the dispersion prepared in Example 1 are shown below.
[0022] Figure 5 This is the gel permeation chromatography curve of the dispersion coating film prepared in Example 2.
[0023] Figure 6 This is a graph showing the particle size test results of the dispersion prepared in Example 3.
[0024] Figure 7 This is a graph showing the particle size test results of the dispersion prepared in Example 5. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1 A water-based fluorinated hybrid acrylic resin dispersion comprises the following raw materials in parts by weight: Epoxy resin: Sanmu brand E-51 epoxy resin, 132 parts; Hydrophilic monomers: 2,2-dimethylolpropionic acid and 2-2 dimethylolbutanoic acid account for 17 and 22 parts respectively; Unsaturated fatty acids: linoleic acid, 62 parts; Glycidyl methacrylate: 18 parts; Tertiary amine catalyst: tetrabutylammonium bromide, 1 part; Vinyl fluoride monomer: vinyloxyethyl perfluorooctanoate, 30 parts; Vinyl soft monomer: butyl acrylate and n-octyl acrylate, accounting for 80 and 30 parts respectively; Vinyl hard monomer: methyl methacrylate, styrene, 125, 5 parts respectively; Initiator: azobisisobutyronitrile, 10 parts; Solvent: propylene glycol methyl ether, 223 parts; Dispersant: deionized water, 744 parts; Neutralizer: N,N-dimethylethanolamine, 25 parts.
[0027] The preparation process of the aqueous fluorinated hybrid acrylic resin dispersion is as follows: (1) Epoxy resin according to the formula was weighed and placed in a reactor at 130°C, and the air in the reactor was replaced with N2. After the temperature stabilized, hydrophilic monomer and tertiary amine catalyst were added and the reaction was carried out at a constant temperature for 3 hours; (2) slowly adding unsaturated fatty acid and glycidyl methacrylate to (1), controlling the dropping time to be 30 min, and then continuing the reaction for 3 h to obtain a vinyl epoxy resin prepolymer; (3) Weighing vinyl fluoride monomer, vinyl soft monomer, vinyl hard monomer and initiator according to the formula, and mixing them uniformly by ultrasonication to obtain a monomer mixture; (4) Cooling the epoxy resin prepolymer obtained in step (2) to 55°C, adding a co-solvent and stirring at a constant temperature for 30 minutes until the mixture is uniformly mixed; then raising the temperature to 95°C, dripping the monomer mixture obtained in step (3), controlling the total dripping time to be 3.5 hours, and keeping the temperature for 4 hours after the dripping is completed, to obtain a water-based fluorinated hybrid acrylic resin; (5) The aqueous fluorinated hybrid acrylic resin obtained in step (4) was cooled to 70° C., a neutralizing agent was added, the pH of the system was adjusted to 8.5, and the mixture was rapidly stirred for 35 min. Then, deionized water was slowly added and dispersed at high speed for 1.5 h. The mixture was filtered to obtain an aqueous fluorinated hybrid acrylic resin dispersion having a solid content of 35%.
[0028] The epoxy resin modified waterborne acrylic resin dispersion prepared in Example 1 was dehydrated and dried, and infrared spectroscopy (FT-IR) was performed. The results are shown in Figure 1 , 2928 cm in the infrared spectrum -1 and 2855cm -1 The CH stretching vibration absorption peak is 1727cm -1 It is the C=O stretching vibration absorption peak, the CF bond infrared characteristic absorption peaks appear at 1378cm-1, 1296cm-1, and 697cm-1, and the methylene CH infrared spectrum absorption peak appears at 2928cm-1, indicating that the DFMA monomer successfully copolymerizes with the acrylate monomer. Figure 2 This is a thermogravimetric test curve of the dispersion coating prepared in this example after drying. It can be seen from the figure that the temperature at which the resin loses 10% of its weight is 344°C, and the thermal stability is good. Figure 3 The DSC curve of the dispersion resin coating after drying is shown in Figure 1. The glass transition temperature of the resin is around 10.7°C. Figure 4 To prepare the particle size distribution of the dispersion, it can be seen that the particle size distribution of the prepared dispersion is uniform, and 90% of the particle size distribution is below 164nm.
[0029] Example 2 A water-based fluorinated hybrid acrylic resin dispersion comprises the following raw materials in parts by weight: Epoxy resin: BE188EL epoxy resin, 180 parts; Hydrophilic monomer: 2-2 dihydroxymethyl butyric acid accounts for 57 parts respectively; Unsaturated fatty acids: linoleic acid, 94 parts Glycidyl methacrylate: 31 parts; Tertiary amine catalyst: tetrabutylammonium bromide, 3 parts; Vinyl fluoride monomer: vinyloxyethyl perfluorooctanoate, 80 parts Vinyl soft monomer: butyl acrylate, 180 parts; Vinyl hard monomers: methyl methacrylate and styrene, accounting for 135 and 65 parts respectively; Initiator: azobisisoheptanonitrile, 27 parts; Solvent: propylene glycol butyl ether, 396 parts; Dispersant: deionized water, 908 parts; Neutralizing agent: N, N-dimethylethanolamine, 45 parts.
[0030] The preparation process of the aqueous fluorinated hybrid acrylic resin dispersion is as follows: (1) Weigh the epoxy resin according to the formula and place it in a reactor at 150°C. Replace the air in the reactor with N2. After the temperature stabilizes, add the hydrophilic monomer and tertiary amine catalyst and react at a constant temperature for 2 hours. (2) slowly adding unsaturated fatty acid and glycidyl methacrylate to (1), controlling the dropping time to be 25 min, and then continuing the reaction for 2.5 h to obtain a vinyl epoxy resin prepolymer; (3) Weighing vinyl fluoride monomer, vinyl soft monomer, vinyl hard monomer and initiator according to the formula, and mixing them uniformly by ultrasonication to obtain a monomer mixture; (4) Cooling the epoxy resin prepolymer obtained in step (2) to 75°C, adding a co-solvent and stirring at a constant temperature for 20 minutes until the mixture is uniformly mixed; then heating to 90°C, dripping the monomer mixture obtained in step (3), controlling the total dripping time to be 4.0 hours, and keeping the temperature for 3 hours after the dripping is completed to obtain a water-based fluorinated hybrid acrylic resin; (5) The aqueous fluorinated hybrid acrylic resin obtained in step (4) was cooled to 70° C., a neutralizing agent was added, the pH of the system was adjusted to 7.5, and the mixture was rapidly stirred for 35 min. Then, deionized water was slowly added and dispersed at high speed for 1.5 h. The mixture was filtered to obtain an aqueous fluorinated hybrid acrylic resin dispersion having a solid content of 40%.
[0031] The molecular weight of the dispersion resin prepared in this example is tested as follows Figure 5It can be seen that the resin molecular weight presents a wide distribution state, and the weight average molecular weight Mw is 42773.
[0032] Example 3 A water-based fluorinated hybrid acrylic resin dispersion comprises the following raw materials in parts by weight: Epoxy resin: BE188EL epoxy resin, 155 parts; Hydrophilic monomer: 2-2 dihydroxymethyl butyric acid accounts for 40 parts respectively; Unsaturated fatty acids: linoleic acid, 70 parts Glycidyl methacrylate: 25 parts; Tertiary amine catalyst: tetrabutylammonium bromide, 2 parts; Vinyl fluoride monomer: vinyloxyethyl perfluorooctanoate, 70 parts Vinyl soft monomer: butyl methacrylate and isooctyl acrylate, accounting for 100 and 47 parts respectively; Vinyl hard monomer: methyl methacrylate, styrene, acrylonitrile, accounting for 105, 65, and 30 parts respectively; Initiator: azobisisobutyronitrile, 22 parts; Solvent: propylene glycol butyl ether and propylene glycol methyl ether, accounting for 190 and 100 parts respectively; Dispersant: deionized water, 814 parts; Neutralizer: N,N-dimethylethanolamine, 34 parts.
[0033] The preparation process of the aqueous fluorinated hybrid acrylic resin dispersion is as follows: (1) Epoxy resin according to the formula was weighed and placed in a reactor at 140°C, and the air in the reactor was replaced with N2. After the temperature stabilized, hydrophilic monomer and tertiary amine catalyst were added and the reaction was carried out at a constant temperature for 2.5 hours; (2) slowly adding unsaturated fatty acid and glycidyl methacrylate to (1), controlling the dropping time to be 20 min, and then continuing the reaction for 2.5 h to obtain a vinyl epoxy resin prepolymer; (3) Weighing vinyl fluoride monomer, vinyl soft monomer, vinyl hard monomer and initiator according to the formula, and mixing them uniformly by ultrasonication to obtain a monomer mixture; (4) Cooling the epoxy resin prepolymer obtained in step (2) to 65°C, adding a co-solvent and stirring at a constant temperature for 20 minutes until the mixture is uniformly mixed; then heating to 95°C, dripping the monomer mixture obtained in step (3), controlling the total dripping time to be 3.5 hours, and keeping the temperature for 3 hours after the dripping is completed to obtain a water-based fluorinated hybrid acrylic resin; (5) The aqueous fluorinated hybrid acrylic resin obtained in step (4) was cooled to 60° C., a neutralizing agent was added, the pH of the system was adjusted to 8, and the mixture was rapidly stirred for 30 min. Then, deionized water was slowly added and dispersed at high speed for 1 h. The mixture was filtered to obtain an aqueous fluorinated hybrid acrylic resin dispersion having a solid content of 38%.
[0034] The particle size distribution of the dispersion prepared in this example is as follows Figure 6 , it can be seen that the particle size distribution of the dispersion is relatively uniform, with 90% of the particle size distribution below 167nm.
[0035] Example 4 A water-based fluorinated hybrid acrylic resin dispersion comprises the following raw materials in parts by weight: Epoxy resin: BE188EL epoxy resin, 160 parts; Hydrophilic monomer: 2-2 dimethylol propionic acid accounts for 38 parts respectively; Unsaturated fatty acids: linoleic acid, 71 parts Glycidyl methacrylate: 27 parts; Tertiary amine catalyst: tetrabutylammonium bromide, 2.5 parts; Vinyl fluoride monomer: vinyloxyethyl perfluorooctanoate, 100 parts Vinyl soft monomer: butyl methacrylate and isooctyl acrylate, accounting for 100 and 47 parts respectively; Vinyl hard monomer: methyl methacrylate, styrene, acrylonitrile, accounting for 85, 65, and 30 parts respectively; Initiator: azobisisobutyronitrile, 22 parts; Solvent: propylene glycol butyl ether and propylene glycol methyl ether, accounting for 130 and 160 parts respectively; Dispersant: deionized water, 815 parts; Neutralizer: N,N-dimethylethanolamine, 35 parts.
[0036] The preparation process of the aqueous fluorinated hybrid acrylic resin dispersion is as follows: (1) Epoxy resin according to the formula was weighed and placed in a reactor at 140°C, and the air in the reactor was replaced with N2. After the temperature stabilized, hydrophilic monomer and tertiary amine catalyst were added and the reaction was carried out at a constant temperature for 2.5 hours; (2) slowly adding unsaturated fatty acid and glycidyl methacrylate to (1), controlling the dropping time to be 20 min, and then continuing the reaction for 2.5 h to obtain a vinyl epoxy resin prepolymer; (3) Weighing vinyl fluoride monomer, vinyl soft monomer, vinyl hard monomer and initiator according to the formula, and mixing them uniformly by ultrasonication to obtain a monomer mixture; (4) Cooling the epoxy resin prepolymer obtained in step (2) to 65°C, adding a co-solvent and stirring at a constant temperature for 20 minutes until the mixture is uniformly mixed; then heating to 95°C, dripping the monomer mixture obtained in step (3), controlling the total dripping time to be 3.5 hours, and keeping the temperature for 3 hours after the dripping is completed to obtain a water-based fluorinated hybrid acrylic resin; (5) The aqueous fluorinated hybrid acrylic resin obtained in step (4) was cooled to 70° C., a neutralizing agent was added, the pH of the system was adjusted to 7.5, and the mixture was rapidly stirred for 30 min. Then, deionized water was slowly added and dispersed at high speed for 1 h. The mixture was filtered to obtain an aqueous fluorinated hybrid acrylic resin dispersion having a solid content of 39%.
[0037] Example 5 A water-based fluorinated hybrid acrylic resin dispersion comprises the following raw materials in parts by weight: 132-180 parts of epoxy resin, 39-57 parts of hydrophilic monomer, 62-94 parts of unsaturated fatty acid, 18-31 parts of glycidyl methacrylate, 30-100 parts of vinyl fluoride monomer, 80-180 parts of vinyl soft monomer, 110-200 parts of vinyl hard monomer, 1-3 parts of tertiary amine catalyst, 223-396 parts of solvent, 10-27 parts of initiator, 25-45 parts of neutralizer and deionized water; Epoxy resin: BE188EL epoxy resin, 160 parts; Hydrophilic monomer: 2-2 dimethylol propionic acid accounts for 38 parts respectively; Unsaturated fatty acids: linoleic acid, 74 parts Glycidyl methacrylate: 30 parts; Tertiary amine catalyst: tetrabutylammonium bromide, 2.5 parts; Vinyl fluoride monomer: vinyloxyethyl perfluorooctanoate, 95 parts Vinyl soft monomer: butyl acrylate and isooctyl acrylate, accounting for 50 and 30 parts respectively; Vinyl hard monomer: methyl methacrylate, 110 parts; Initiator: azobisisobutyronitrile, 15 parts; Solvent: propylene glycol butyl ether and propylene glycol methyl ether, accounting for 130 and 121 parts respectively; Dispersant: deionized water, 839 parts; Neutralizing agent: triethylamine and N,N-dimethylethanolamine, accounting for 20 and 14 parts respectively.
[0038] The preparation process of the aqueous fluorinated hybrid acrylic resin dispersion is as follows: (1) Weigh the epoxy resin according to the formula and place it in a reactor at 140°C. Replace the air in the reactor with N2. After the temperature stabilizes, add the hydrophilic monomer and tertiary amine catalyst and react at a constant temperature for 3 hours. (2) slowly adding unsaturated fatty acid and glycidyl methacrylate to (1), controlling the dropping time to be 27 min, and then continuing the reaction for 2 h to obtain a vinyl epoxy resin prepolymer; (3) Weighing vinyl fluoride monomer, vinyl soft monomer, vinyl hard monomer and initiator according to the formula, and mixing them uniformly by ultrasonication to obtain a monomer mixture; (4) Cooling the epoxy resin prepolymer obtained in step (2) to 55°C, adding a co-solvent and stirring at a constant temperature for 20 minutes until the mixture is uniformly mixed; then raising the temperature to 87°C, dripping the monomer mixture obtained in step (3), controlling the total dripping time to be 5.5 hours, and keeping the temperature for 4 hours after the dripping is completed, to obtain a water-based fluorinated hybrid acrylic resin; (5) The aqueous fluorinated hybrid acrylic resin obtained in step (4) was cooled to 68° C., a neutralizing agent was added, the pH of the system was adjusted to 8.5, and the mixture was rapidly stirred for 30 min. Then, deionized water was slowly added and dispersed at high speed for 1 h. The mixture was filtered to obtain an aqueous fluorinated hybrid acrylic resin dispersion having a solid content of 35%.
[0039] The particle size distribution of the dispersion prepared in this example is as follows Figure 7 , it can be seen that the particle size distribution of the dispersion is relatively uniform, with 90% of the particle size distribution below 182nm.
[0040] Test Case To further illustrate the aqueous fluorinated hybrid acrylic resin dispersion disclosed in the present invention, the present invention also conducted corresponding tests on the aqueous fluorinated hybrid acrylic resin dispersion and coating film prepared in Examples 1 to 5, and the test method is as follows: Dispersion particle size test: The aqueous fluorinated hybrid acrylic resin dispersion was diluted into deionized water, and the dispersion particle size and its distribution were tested using a laser particle size analyzer.
[0041] Resin storage and transportation stability test: Place the water-based fluorinated hybrid acrylic resin dispersion sample in a 50°C oven and keep it at a constant temperature for 1 month. Take it out and place it at room temperature for observation. If no gel or separation occurs, it passes the test.
[0042] Determination of adhesion of resin coating film: The adhesion of the dispersion coating film prepared in the example was measured according to the method of GB / T9286-1998.
[0043] Determination of surface drying time and actual drying time of coating film: The aqueous fluorinated hybrid acrylic resin dispersion prepared in the example was evenly applied on a polytetrafluoroethylene plate, dried at a constant temperature of 25° C. The surface drying time and actual drying time of the coating film were determined according to the method of GB1728-79.
[0044] Acid and alkali resistance test of resin film: Determined according to GB / T 9274 Method A; Resin coating hardness test: According to GB / T6739-2006 standard, the hardness of the coating film is measured by pencil method; Resin coating salt spray resistance test: GB / T1771-2007 standard is used to test the neutral salt spray resistance of resin coatings. If the coating does not bubble or fall off for 336 hours and slight discoloration is allowed, it is considered to have passed the test; Resin coating water resistance test: The resin coating water resistance is tested using the method of GB / T1733-1993. If the coating does not bubble or fall off for 336 hours and slight discoloration is allowed, it is considered to have passed the test. Resin coating performance test table The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An aqueous fluorinated hybrid acrylic resin dispersion, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 132-180 parts of epoxy resin, 39-57 parts of hydrophilic monomer, 62-94 parts of unsaturated fatty acid, 18-31 parts of glycidyl methacrylate, 30-100 parts of vinyl fluoride monomer, 110-180 parts of vinyl soft monomer, 130-200 parts of vinyl hard monomer, 1-3 parts of tertiary amine catalyst, 223-396 parts of solvent, 10-27 parts of initiator, 25-45 parts of neutralizer and 744-908 parts of deionized water.
2. The aqueous fluorinated hybrid acrylic resin dispersion according to claim 1, Features: The epoxy value of the epoxy resin is 0.35-0.55 mol / 100g, and the epoxy resin is E-51 epoxy resin or BE188EL epoxy resin; and the unsaturated fatty acid is linoleic acid.
3. The aqueous fluorinated hybrid acrylic resin dispersion according to claim 1, Features: The hydrophilic monomer is 2,2-dimethylol propionic acid and / or 2,2-dimethylol butyric acid.
4. The aqueous fluorinated hybrid acrylic resin dispersion according to claim 1, Features: The vinyl fluoride monomer is vinyloxyethyl perfluorooctanoate, and its structural formula is: 。 5. The aqueous fluorinated hybrid acrylic resin dispersion according to claim 1, Features: The vinyl soft monomer is selected from one or any combination of butyl methacrylate, butyl acrylate, n-octyl acrylate, lauryl acrylate, isooctyl acrylate, vinyl acetate, isooctyl methacrylate and n-octyl methacrylate; the vinyl hard monomer is selected from one or any combination of methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, benzyl acrylate, phenyl acrylate, styrene, divinyl benzene and acrylonitrile.
6. The aqueous fluorinated hybrid acrylic resin dispersion according to claim 1, Features: The catalyst is tetrabutylammonium bromide; the initiator is azobisisobutyronitrile and / or azobisisoheptanenitrile; the solvent is propylene glycol methyl ether and / or propylene glycol monobutyl ether; and the neutralizer is triethylamine and / or N,N-dimethylethanolamine.
7. A method for preparing an aqueous fluorinated hybrid acrylic resin dispersion according to any one of claims 1 to 6, It is characterized in that The following steps are included: (1) Weigh epoxy resin, hydrophilic monomer and tertiary amine catalyst according to the formula. 2 React under protection; (2) adding unsaturated fatty acid and glycidyl methacrylate dropwise to (1), followed by further reaction to obtain a vinyl epoxy resin prepolymer; (3) Weighing vinyl fluoride monomer, vinyl soft monomer, vinyl hard monomer and initiator according to the formula, and mixing them uniformly by ultrasonication to obtain a monomer mixture; (4) cooling the vinyl epoxy resin prepolymer in step (2), adding a co-solvent, stirring and mixing at a constant temperature to mix evenly; then raising the temperature, adding dropwise the monomer mixture in step (3), and reacting to obtain a water-based fluorinated hybrid acrylic resin; (5) After cooling the aqueous fluorinated hybrid acrylic resin in step (4), a neutralizing agent is added to adjust the pH of the system to 7.5-8.5, and the mixture is stirred evenly. Deionized water is then added to disperse the mixture at high speed, and the mixture is filtered to obtain an aqueous fluorinated hybrid acrylic resin dispersion.
8. The method for preparing the aqueous fluorinated hybrid acrylic resin dispersion according to claim 7, It is characterized in that The reaction temperature in step (1) is 130° C.-150° C., and the reaction time is 2-3 hours; the slow dripping time in step (2) is 20-30 minutes; and the reaction time is continued for 2-3 hours.
9. The method for preparing the aqueous fluorinated hybrid acrylic resin dispersion according to claim 8, It is characterized in that In the step (4), the vinyl epoxy resin prepolymer is first cooled to 55-75°C; after the co-solvent is added, the stirring and mixing time is 20-30 minutes; then the temperature is raised to 85-95°C; the monomer mixture is added dropwise for 3.5-5.5 hours, and the reaction time is 3-5 hours.
10. The method for preparing the aqueous fluorinated hybrid acrylic resin dispersion according to claim 8, Features: In the step (5), the water-based fluorinated hybrid acrylic resin is first cooled to 60-70° C.; the rapid stirring time is 30-35 minutes; the high-speed dispersion time is 1-1.5 hours; and the solid content of the water-based fluorinated hybrid acrylic resin dispersion is 35-40%.