Liquid crystal polymer as well as preparation method and application thereof
By introducing amorphous polymers into the liquid crystal polymer to form a block structure, the problems of low peeling force and poor appearance of liquid crystal polymer film and copper foil are solved, high copper clad peeling force and good appearance are achieved, and stable product performance is improved sex.
Patent Information
- Application Number
- CN202411192999.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The copper-clad peeling force between the liquid crystal polymer film and the low-roughness copper foil is low, and the appearance is poor due to anisotropy, which affects the stability of the product performance.
A specific amount of amorphous polymer is introduced into the liquid crystal polymer, and a block structure is formed through acylation reaction and polycondensation reaction, which regulates the molecular sequence structure and improves the instantaneous fluidity and appearance quality of the film.
The high copper clad peeling force between the liquid crystal polymer film and the high-frequency copper foil is achieved, and the appearance of the film is improved and the performance stability of the product is improved.
Smart Images

Figure CN119060308A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically, to a liquid crystal polymer and a preparation method and application thereof. Background Art
[0002] Liquid crystal polymer (LCP) has excellent high-frequency dielectric properties, processing fluidity, high heat resistance and dimensional stability, and is widely used in the field of electronics and electrical appliances. The 5G commercial era is characterized by higher electromagnetic wave transmission speeds and smaller signal propagation losses, requiring the dielectric constant and dielectric loss of the material to be as small as possible. Liquid crystal polymer is the material that meets these stringent requirements. Therefore, flexible printed circuit boards based on liquid crystal polymer films have become the best material for 5G terminal antennas.
[0003] The high-frequency characteristics of copper foil used as a transmission line, i.e., the transmission loss, depend on the skin effect (surface resistance) and the surface roughness Rz of the copper foil. If the Rz of the copper foil is large, the signal transmission loss is large, i.e., the high-frequency characteristics are poor. The use of low-roughness copper foil can reduce the "skin effect" and thus reduce the transmission loss, but at the same time, it will cause the adhesion strength between the copper foil and the liquid crystal polymer film, i.e., the copper peeling strength is low. How to improve the copper peeling strength between the liquid crystal polymer film and the low-roughness copper foil is a technical difficulty in developing flexible circuit boards using liquid crystal polymer film as a substrate to meet the requirements of high-frequency communications.
[0004] Patent CN107530979A provides a method for manufacturing a metal-clad laminate for a flexible circuit board. The method is to first hot-press a liquid crystal polymer film and a metal foil (such as aluminum foil, etc.), and then select a heat treatment temperature 1 to 50°C higher than the melting point of the LCP film, and control the annealing time to achieve regulation of the surface thickness of the LCP film, thereby improving the adhesion strength between the liquid crystal polymer film and the high-frequency copper foil (Rz = 0.9μm) and reducing the high-frequency transmission loss of the prepared circuit board.
[0005] However, the above patent improves the peeling force by a specific heat treatment process. If the bonding peeling force between the liquid crystal polymer film and the metal foil is improved by improving the liquid crystal polymer itself, the application range of the liquid crystal polymer film can be expanded. Therefore, it is necessary to develop a liquid crystal polymer with high peeling strength with metal foil.
[0006] In addition, it is also worth noting that LCP materials show anisotropy in the molten state due to local order; when the liquid crystal polymer film is prepared by blow molding, the appearance of the liquid crystal polymer film shows heterogeneous characteristics due to the anisotropic characteristics, which affects the appearance. The excellent appearance of the liquid crystal polymer film has a great influence on the performance stability of the products of downstream manufacturers. Summary of the invention
[0007] The primary purpose of the present invention is to overcome the current problems of low peel strength between a liquid crystal polymer film and a low-roughness copper foil or poor appearance of the liquid crystal polymer film, and to provide a liquid crystal polymer.
[0008] A further object of the present invention is to provide a method for preparing the above liquid crystal polymer.
[0009] A further object of the present invention is to provide use of the above liquid crystal polymer in preparing a liquid crystal polymer film.
[0010] A further object of the present invention is to provide a liquid crystal polymer film.
[0011] A further object of the present invention is to provide a method for preparing the above-mentioned liquid crystal polymer film.
[0012] A further object of the present invention is to provide an application of the above-mentioned liquid crystal polymer film in the preparation of a flexible circuit board.
[0013] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0014] A liquid crystal polymer, wherein the liquid crystal polymer resin is obtained by reacting a mixture of hydroxybenzoic acid or its derivative, 2-hydroxy-6-naphthoic acid or its derivative and an amorphous polymer;
[0015] The mass percentage of the amorphous polymer in the mixture is 1 to 5.5%;
[0016] The amorphous polymer is composed of diphenol units and dicarboxylic acid units.
[0017] The addition of a specific amount of amorphous polymers of the present invention can introduce a specific block structure into the liquid crystal polymer, regulate the molecular sequence structure of the liquid crystal polymer, thereby regulating the instantaneous fluidity of the surface layer of the film when the liquid crystal polymer film is hot-pressed with the copper foil, and achieving a high copper-clad peeling force between the liquid crystal polymer film and the high-frequency copper foil. In addition, the block structure brought about by the introduction of the specific amorphous polymer also reduces the inherent rigidity of the LCP molecules, improves the film appearance defects caused by the anisotropy of the LCP material, so that the liquid crystal polymer film prepared by the liquid crystal polymer of the present invention has a good appearance.
[0018] In the present invention, the liquid crystal polymer is obtained by acylation reaction and polycondensation reaction of p-hydroxybenzoic acid, 2-hydroxy-6-naphthoic acid and amorphous polymer.
[0019] Preferably, the solution viscosity of the liquid crystal polymer is 3.0 to 8.0 dL / g.
[0020] The solution viscosity of the liquid crystal polymer can be measured by an Uhlenbeck viscometer at 80°C, with pentafluorophenol as the solvent.
[0021] Preferably, in the mixture, the sum of the masses of p-hydroxybenzoic acid and 2-hydroxy-6-naphthoic acid accounts for 94.5-99%.
[0022] Preferably, in the mixture, the mass ratio of p-hydroxybenzoic acid to 2-hydroxy-6-naphthoic acid is (60-72):(24-36).
[0023] Preferably, in the mixture, the mass proportion of the amorphous polymer is 2-4%. When the mass proportion is adjusted within this range, the high copper-clad peeling force between the liquid crystal polymer film and the high-frequency copper foil obtained by obtaining the liquid crystal polymer is higher.
[0024] Preferably, the solution viscosity of the amorphous polymer is 0.45 to 0.65 dL / g.
[0025] The solution viscosity of the amorphous polymer can be measured by a Uhlenbeck viscometer at 25°C, with chloroform as the solvent.
[0026] Preferably, the diphenol unit is derived from bisphenol A or its ester derivatives; the dicarboxylic acid unit is derived from terephthalic acid or its acyl halide derivatives and isophthalic acid or its acyl halide derivatives.
[0027] More preferably, the bisphenol A or its ester derivative is at least one of bisphenol A, bisphenol A diformate, bisphenol A diacetate or bisphenol A dipropionate.
[0028] More preferably, the terephthalic acid or its acyl halide derivative is at least one of terephthalic acid or terephthaloyl chloride.
[0029] More preferably, the isophthalic acid or its acyl halide derivative is at least one of isophthalic acid and isophthaloyl chloride.
[0030] More preferably, based on the molar percentage of the dicarboxylic acid units, terephthalic acid or its acyl halide derivatives account for 40-60 mol% of the dicarboxylic acid units, and isophthalic acid or its acyl halide derivatives account for 40-60 mol% of the dicarboxylic acid units.
[0031] Further preferably, in terms of molar percentage of the dicarboxylic acid units, terephthalic acid or its acyl halide derivatives account for 40-50 mol% of the dicarboxylic acid units, and isophthalic acid or its acyl halide derivatives account for 50-60 mol% of the dicarboxylic acid units. By regulating the molar ratio within this range, the liquid crystal polymer film obtained by the liquid crystal polymer has a higher high copper peeling force from the high-frequency copper foil.
[0032] Further preferably, in terms of molar percentage of the dicarboxylic acid units, terephthalic acid or its acyl halide derivatives account for 45-50 mol% of the dicarboxylic acid units, and isophthalic acid or its acyl halide derivatives account for 50-55 mol% of the dicarboxylic acid units. When the molar ratio is adjusted within this range, the liquid crystal polymer film obtained by the liquid crystal polymer has a higher high copper peeling force from the high-frequency copper foil.
[0033] The method for preparing the above-mentioned liquid crystal polymer comprises the following steps:
[0034] The liquid crystal polymer is obtained by using p-hydroxybenzoic acid, 2-hydroxy-6-naphthoic acid and amorphous polymer as raw materials, carrying out an acylation reaction in the presence of an acylating agent, and then carrying out a polycondensation reaction.
[0035] Preferably, the acylating agent is acetic anhydride.
[0036] Preferably, the reaction temperature of the acylation reaction is 120-180° C., and the reaction time is 0.5-6 hours.
[0037] Preferably, the temperature of the polycondensation reaction is 200-400° C. and the pressure is below 10 kPa.
[0038] Preferably, the polycondensation reaction is carried out in a reactor, and the reaction is terminated when the power of the stirring paddle of the reactor rises to 1-10 kW.
[0039] The application of the above liquid crystal polymer in the preparation of liquid crystal polymer film also falls within the protection scope of the present invention.
[0040] A liquid crystal polymer film is prepared from the liquid crystal polymer.
[0041] Preferably, the crystallinity of the liquid crystal polymer film is 25-50%.
[0042] Preferably, the transient shear stress of the liquid crystal polymer film is 90-260Pa.
[0043] The method for preparing the above-mentioned liquid crystal polymer film comprises the following steps:
[0044] The liquid crystal polymer is subjected to film blowing to obtain a liquid crystal polymer original film, and then the liquid crystal polymer original film is hot-pressed and laminated with aluminum foil to obtain an LCP / Al laminate; after the LCP / Al laminate passes through a high-temperature cyclization furnace, the aluminum foil is peeled off to obtain a liquid crystal polymer film.
[0045] The application of the above-mentioned liquid crystal polymer film in the preparation of flexible circuit boards is also within the protection scope of the present invention.
[0046] A flexible circuit board comprises the above-mentioned liquid crystal polymer film.
[0047] Preferably, the flexible circuit board further comprises a copper foil bonded to the liquid crystal polymer film.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] The present invention introduces a block structure derived from a specific amount of amorphous polymer into the liquid crystal polymer to regulate the molecular sequence structure of the liquid crystal polymer, thereby regulating the instantaneous fluidity of the surface layer of the liquid crystal polymer film when the liquid crystal polymer film is hot-pressed with the copper foil, thereby achieving a high copper-clad peeling force between the liquid crystal polymer film and the high-frequency copper foil. At the same time, the liquid crystal polymer film prepared by the liquid crystal polymer of the present invention also has a good appearance. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 Schematic diagram of the preparation process of liquid crystal polymer film. DETAILED DESCRIPTION
[0051] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.
[0052] Some of the reagents selected in the embodiments and comparative examples of the present invention are described as follows:
[0053] Amorphous polymer 1#: Homemade, the preparation method is as follows: the purified bisphenol A diacetate, terephthalic acid, and isophthalic acid are fully dried at 90°C, and then bisphenol A diacetate, terephthalic acid, and isophthalic acid are added into the reactor in a molar ratio of 50:25:25, and vacuumed and filled with nitrogen to ensure that the air in the reactor is discharged. Slowly heat to 120°C and keep warm for 30 minutes to discharge moisture. Slowly heat to 240°C under nitrogen protection, keep warm until acetic acid distills out, maintain vacuum, react until acetic acid no longer distills out, then quickly heat to 335°C, vacuum and stir, stop stirring after a period of reaction, and obtain amorphous polymer 1#. During the reaction, the pressure in the reactor needs to be maintained at 0.6 atmospheres. The solution viscosity of the obtained amorphous polymer is 0.56dL / g.
[0054] Amorphous polymer 2#: The preparation method is basically the same as that of amorphous polymer 1#, except that the molar ratio of the three monomers of bisphenol A diacetate, terephthalic acid, and isophthalic acid is 50:30:20.
[0055] Amorphous polymer 3#: The preparation method is basically the same as that of amorphous polymer 1#, except that the molar ratio of the three monomers of bisphenol A diacetate, terephthalic acid, and isophthalic acid is 50:20:30.
[0056] Amorphous polymer 4#: The preparation method is basically the same as that of amorphous polymer 1#, except that the molar ratio of the three monomers of bisphenol A diacetate, terephthalic acid, and isophthalic acid is 50:22.5:27.5.
[0057] Unless otherwise specified, the raw materials used for the above-mentioned amorphous polymers (such as bisphenol A diacetate, terephthalic acid, isophthalic acid) are all the same commercially available products.
[0058] Unless otherwise specified, the components (eg, hydroxybenzoic acid, 2-hydroxy-6-naphthoic acid) used in the parallel examples and comparative examples are all the same commercially available products.
[0059] The liquid crystal polymers of the embodiments and comparative examples were prepared by the following preparation method:
[0060] Weigh p-hydroxybenzoic acid (HBA), 2-hydroxy-6-naphthoic acid (HNA) and amorphous polymer (if any) in the formula, and then throw them together into a reaction vessel containing acetic anhydride acylation dosage. Then place the reactor in a 240℃ salt bath pot for reflux for 2h, and start to extract the reaction by-product acetic acid. After the acylation reaction is completed, heat the reactor to 300℃ at a heating rate of 2.5℃ / min, discharge acetic acid and unreacted raw material small molecules from the distillation column, and then reduce the internal pressure of the reactor to below 10kPa, maintain this pressure, discharge the material and pelletize to obtain liquid crystal polymer.
[0061] Preparation of liquid crystal polymer film: The liquid crystal polymer of each embodiment or comparative example is subjected to film blowing to obtain a liquid crystal polymer original film, and then the liquid crystal polymer original film is hot-pressed and laminated with aluminum foil to obtain an LCP / Al laminate. After the laminate is passed through a high-temperature cyclization furnace, the aluminum foil is peeled off to obtain a liquid crystal polymer film. The schematic diagram of the preparation process is shown in FIG. Figure 1 shown.
[0062] The performance of the liquid crystal polymers provided in the embodiments and comparative examples of the present invention was measured according to the following test methods:
[0063] 1) Melting point of resin: measured by DSC 200F3 manufactured by NETZSCH Company, with a heating rate of 20°C / min, heating to 30°C above the melting point and staying for 5 minutes to eliminate the thermal history, and taking the curve of the second heating to obtain the melting point T m .
[0064] 2) Film transient fluidity: The transient shear stress is used for qualitative characterization and the test is performed using a rotational rheometer (Discovery DHR 2, TA Co., Ltd). The liquid crystal polymer film sample is kept at this temperature for 3 minutes before the measurement is started. The test temperature is the copper cladding pressing temperature, i.e. the film melting point, and the test frequency is 10 rad / s.
[0065] 3) Thin film copper peeling strength: The liquid crystal polymer film and the high-frequency copper foil (Rz = 1.0 μm) were hot-pressed near the melting point of the film to obtain a copper-clad laminate at a composite pressure of 3 MPa. Five strips with a width of 10 mm were cut from the copper-clad laminate to test the copper peeling strength of the copper-clad laminate. The test standard was in accordance with GB / T 13542.2-2009.
[0066] 4) Evaluation of the appearance of liquid crystal polymer film: Place the formed liquid crystal polymer film under strong light to observe the appearance of the liquid crystal polymer film. The forming process is: the length of the liquid crystal polymer film (about 1 meter) that can be prepared by one rotation of the fluid flow control pump is used as the basis for the evaluation of the film appearance; the number of white spots on the surface of the film is used as the basis for judgment: "0≤Number of defects≤3" is rated as excellent, "3<Number of defects≤8" is rated as qualified, "8<Number of defects≤15" is rated as unqualified, and "Number of defects>15" is rated as poor.
[0067] Examples 1 to 9
[0068] Examples 1 to 9 provide a series of liquid crystal polymers, whose formulations are shown in Table 1.
[0069] Table 1 Formulas of Examples 1 to 9 (parts by weight)
[0070]
[0071] Comparative Examples 1-2
[0072] Comparative Examples 1-2 provide a series of liquid crystal polymers, whose formulas are shown in Table 2.
[0073] Table 2 Formula of Comparative Examples 1 to 2 (parts by weight)
[0074]
[0075] Comparative Example 3
[0076] This comparative example provides a liquid crystal polymer composition, and the preparation process is as follows:
[0077] 1) Preparation of liquid crystal polymer is basically the same as in Example 1, except that amorphous polymer 1# is not added.
[0078] 2) preparing a liquid crystal polymer composition, mixing the liquid crystal polymer prepared in step 1) with amorphous polymer 1# at a mass ratio of 98:2, feeding into a twin-screw extruder, and kneading and granulating at a temperature 30°C higher than the melting point of the liquid crystal polymer to obtain a liquid crystal polymer composition.
[0079] The properties of the liquid crystal polymers of the embodiments and comparative examples were measured according to the above-mentioned test methods. The test results are shown in Table 3.
[0080] Table 3 Test results of liquid crystal polymer properties of various embodiments and comparative examples
[0081]
[0082] From Table 3, we can see that:
[0083] The peeling strength of the liquid crystal polymer films of Examples 1 to 9 in the copper peeling test are all above 0.65 N / mm, and the appearance grades are all excellent or qualified, indicating that the liquid crystal polymer film of the present invention has high copper peeling strength with the high-frequency copper foil and has a good appearance.
[0084] The amount of amorphous polymer added during the preparation of the liquid crystal polymer in Comparative Examples 1 and 2 is too low or too high, and the resulting liquid crystal polymer film has poor peeling strength from the high-frequency copper foil, and the appearance is unqualified or poor. The film formed from the liquid crystal polymer composition of Comparative Example 3 has a lower peeling strength than that of Example 1, and the appearance is unqualified.
[0085] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A liquid crystal polymer, characterized in that: The liquid crystal polymer resin is obtained by reacting a mixture of hydroxybenzoic acid or its derivatives, 2-hydroxy-6-naphthoic acid or its derivatives and an amorphous polymer; The mass percentage of the amorphous polymer in the mixture is 1 to 5.5%; The amorphous polymer is composed of diphenol units and dicarboxylic acid units.
2. The liquid crystal polymer according to claim 1, characterized in that: In the mixture, the mass ratio of p-hydroxybenzoic acid to 2-hydroxy-6-naphthoic acid is (60-72):(24-36).
3. The liquid crystal polymer according to claim 1, characterized in that: In the mixture, the mass proportion of the amorphous polymer is 2-4%.
4. The liquid crystal polymer according to claim 1, characterized in that: The diphenol unit is derived from bisphenol A or its ester derivatives; the dicarboxylic acid unit is derived from terephthalic acid or its acyl halide derivatives and isophthalic acid or its acyl halide derivatives.
5. The liquid crystal polymer resin according to claim 4, characterized in that: In terms of molar percentage of the dicarboxylic acid units, terephthalic acid or its acyl halide derivatives account for 40-60 mol% of the dicarboxylic acid units, and isophthalic acid or its acyl halide derivatives account for 40-60 mol% of the dicarboxylic acid units.
6. The method for preparing a liquid crystal polymer according to any one of claims 1 to 5, characterized in that: The steps include: The liquid crystal polymer is obtained by using p-hydroxybenzoic acid, 2-hydroxy-6-naphthoic acid and amorphous polymer as raw materials, carrying out an acylation reaction in the presence of an acylating agent, and then carrying out a polycondensation reaction.
7. Use of the liquid crystal polymer according to any one of claims 1 to 5 in the preparation of liquid crystal polymer films.
8. A liquid crystal polymer film, characterized in that: It is prepared by the liquid crystal polymer described in any one of claims 1 to 5.
9. Use of the liquid crystal polymer film according to claim 8 in the preparation of flexible circuit boards.
10. A flexible circuit board, characterized in that: Comprising the liquid crystal polymer film as claimed in claim 8.
Citation Information
Patent Citations
Aromatic liquid crystal polyester compositions with excellent toughness
CN101497795A
Thermotropic liquid crystal block polyarylate as well as preparation and application thereof
CN112979934A
Liquid crystal polyester as well as preparation method and application thereof
CN113912825A
LCP (Liquid Crystal Polymer) resin composition as well as preparation method and application thereof
CN114685957A
Liquid crystal polyester composition as well as preparation method and application thereof
CN117820828A
Cited By
Liquid crystal polymer and preparation method therefor and use thereof
WO2026046037A1