Flame-retardant polymer foam material and preparation method thereof

Through the combined preparation method of polystyrene, SBS, modified nano-silica and special additives, the problems of flammable and low impact strength of polystyrene foamed materials are solved, and efficient flame retardant and smoke inhibition are achieved. Impact resistance improves the safety and application value of the material.

CN119060465APending Publication Date: 2024-12-03BAOYUANHUI NEW MATERIAL TECHNOLOGY (SUZHOU) CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411312932.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Polystyrene foaming materials are flammable and have low impact resistance. The existing flame retardants release toxic smoke, which hinder personnel evacuation and fire extinguishing. The bubble cells are prone to rupture, which poses safety hazards and insufficient performance.

Method used

The mixed preparation method of polystyrene, SBS, modified nano-silica and special additives is used to foam through twin-screw extrusion and expansion extruder to prepare flame retardant polymer foaming material, and modified nano-sized Silica and additives improve the mechanical strength and impact resistance of the material, and additives have a synergistic effect to improve flame retardant and smoke suppression performance.

Benefits of technology

The foamed material produced has light weight, good thermal insulation performance, small cell size and excellent performance. It has stable and efficient flame retardant and smoke resistance and impact resistance, which significantly improves the safety and application value of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005051229400000031
    Figure BDA0005051229400000031
  • Figure BDA0005051229400000032
    Figure BDA0005051229400000032
  • Figure BDA0005051229400000041
    Figure BDA0005051229400000041
Patent Text Reader

Abstract

The invention discloses a flame-retardant polymer foaming material and a preparation method thereof, and belongs to the technical field of foaming materials. Comprising the following raw materials in parts by weight: 60-80 parts of polystyrene, 10-20 parts of styrene-butadiene-styrene, 4-8 parts of modified nano silicon dioxide, 5-15 parts of an auxiliary agent and 3-5 parts of a lubricant. The prepared foaming material takes polystyrene as a matrix, so that the material is endowed with light weight and thermal insulation performance; the SBS and the polystyrene are blended, so that the impact resistance of the foaming material can be improved; wherein the modified nano silicon dioxide has better compatibility with a polystyrene matrix, can improve the mechanical strength of the foaming material, and can also be used as a nucleating agent; wherein the auxiliary agent belongs to macromolecules and not only serves as a foaming agent, but also various groups in the auxiliary agent can achieve a synergistic effect, so that the flame retardance, smoke suppression and impact resistance of the material are remarkably improved, and the material is long-lasting and stable in performance and not prone to falling off. Therefore, the invention has important application value in the technical field of foaming materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foaming materials, and in particular, relates to a flame retardant polymer foaming material and a preparation method thereof. Background Art

[0002] Foaming material is a porous material with many tiny pores. It has the characteristics of light weight, heat insulation, sound absorption, shock absorption, etc., and its dielectric properties are better than the base resin. It is widely used in the automotive, packaging, electronic appliances, building materials and other industries. According to the hardness of the foaming material, it can be divided into three types: soft, hard and semi-hard. Common polymer foaming materials include polyurethane (PU) foam, polystyrene (PS) foam, polyolefin foam, polyvinyl chloride (PVC) foam, phenolic foam, epoxy resin foam, etc. Among them, polystyrene is a polymer with styrene as a monomer. PS has the advantages of good light transmittance, excellent electrical insulation, and good chemical stability. The foaming material made of polystyrene is light, has low thermal conductivity, low water absorption, and good electrical properties. It has the advantages of heat insulation, shock absorption, sound insulation, low cost, simple and feasible production and molding process equipment, and can be made into products of various shapes and different densities. Therefore, it has been rapidly developed and widely used in the construction, automobile, packaging, aerospace and home appliances industries.

[0003] Polystyrene foam material is an excellent thermal insulation material, and also a high molecular polymer. It has a low oxygen index and is easy to burn. It will burn violently when encountering an open flame, posing a great safety hazard. The most common method to improve the flame retardant properties of polystyrene foam materials is to add flame retardants. The common flame retardants on the market are halogen flame retardants, but these halogen flame retardants release a lot of smoke and toxic and harmful hydrogen halide gas when they burn. Since their diffusion speed is much faster than the flame diffusion speed, they can easily hinder the rapid evacuation of personnel and fire fighting, causing serious impact and loss on people's lives and property safety. In addition, polystyrene foam materials have low impact strength, slow recovery speed after high-intensity impact, and easy rupture of bubbles. Therefore, it is urgent to solve the above problems to meet the higher demands in the field of foam material technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a flame retardant polymer foam material and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a flame retardant polymer foam material comprises the following steps:

[0007] Polystyrene (PS), styrene-butadiene-styrene (SBS), modified nano-silica, additives and lubricants are mixed, added into a twin-screw extruder, melt-blended, extruded, and then injected into an expansion extruder for foaming. After the foaming is completed, a flame-retardant polymer foam material is obtained.

[0008] SBS is a block copolymer of styrene and butadiene. After being heated, the material has good fluidity and is easy to process and shape. It can improve the impact resistance of the foam material to a certain extent.

[0009] Furthermore, the raw materials are calculated in parts by weight as follows: 60-80 parts of polystyrene, 10-20 parts of styrene-butadiene-styrene, 4-8 parts of modified nano-silicon dioxide, 5-15 parts of additives, and 3-5 parts of lubricants.

[0010] Furthermore, the lubricant is one of paraffin and stearamide fatty acid.

[0011] Furthermore, the modified nano-silicon dioxide is prepared by the following steps:

[0012] The nano-silica was mixed with an ethanol aqueous solution, added to a magnetic stirring device, a magnet was added, stirring was started, and the mixture was dispersed for 35 minutes to uniformly disperse the nano-silica in the ethanol aqueous solution. The device was evacuated, N2 gas was introduced, and γ-glycidyloxypropyltrimethoxysilane (silane coupling agent KH-560) was added. The temperature was controlled at 80°C, and the reaction was kept warm for 4 hours. After the reaction was completed, the mixture was filtered, washed with ethanol, and dried in a vacuum drying oven for 2 hours to obtain modified nano-silica.

[0013] Furthermore, the usage ratio of the nano-silica, the ethanol aqueous solution, and γ-glycidyloxypropyltrimethoxysilane is 1.0 g:100 mL:6.5 g.

[0014] There are many -OH groups on the surface of nano-silica, which react with KH-560 to obtain modified nano-silica. Compared with ordinary nano-silica, it has better compatibility with the polystyrene matrix and is easier to disperse. It can not only improve the mechanical strength of the foamed material, but also act as a nucleating agent to reduce the activation energy required for nucleation, so that the pores change from homogeneous nucleation to heterogeneous nucleation, making the pore size smaller, the pores more numerous, and the distribution more uniform, making the performance of the foamed material better.

[0015] Furthermore, the auxiliary agent is prepared by the following steps:

[0016] S1. In a three-necked flask equipped with a stirring device, diethylenetriamine, stearic acid and toluene were mixed and stirred evenly, dicyclohexylcarbodiimide (DCC, dehydrating agent) was added, and the device was placed in a water bath, and the reaction was kept at 50° C. for 3 hours. After the reaction was completed, the mixture was filtered, the solvent was removed by rotary evaporation, and the mixture was washed with anhydrous ethanol for 2-3 times, and vacuum dried to obtain intermediate 1; the ratio of diethylenetriamine, stearic acid, toluene and dicyclohexylcarbodiimide was 11.4 g: 28.4 g: 150 mL: 20.6 g;

[0017] The carboxyl group on stearic acid and the amino group on diethylenetriamine undergo an amidation reaction. Under the action of dicyclohexylcarbodiimide, the reaction can be carried out under relatively mild conditions. By controlling the molar ratio of the two to be close to 1:1 and a slight excess of diethylenetriamine, only one amino group on diethylenetriamine participates in the reaction to obtain intermediate 1. The specific reaction process is shown below:

[0018]

[0019] S2. Add intermediate 1, diethylphosphoacetic acid, dicyclohexylcarbodiimide and toluene to a three-necked flask equipped with a stirring device, stir and mix well, place in a water bath at 55°C, and heat in a water bath for 6 hours. After the reaction is completed, filter, distill under reduced pressure to remove the solvent, and then purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two is 5:1), and remove the eluent by rotary evaporation to obtain intermediate 2; the ratio of the amount of intermediate 1, diethylphosphoacetic acid, dicyclohexylcarbodiimide and toluene is 36.9g:19.6g:20.6g:150mL;

[0020] Under the action of dicyclohexylcarbodiimide, intermediate 1 undergoes an amidation reaction with diethylphosphoacetic acid to obtain intermediate 2. The specific reaction process is as follows:

[0021]

[0022] S3. After cyanuric chloride and toluene are stirred and mixed uniformly in a three-necked flask under an ice bath, intermediate 2 is added to the reaction system, and sodium hydroxide solution (mass fraction 4%) is slowly added dropwise, and the reaction is carried out while dropping, and the reaction temperature is controlled at 0°C. After the dropwise addition is completed, the reaction is continued for 2h. After the reaction is completed, the mixture is filtered, and the solvent is removed by distillation under reduced pressure. The mixture is washed with chloroform for 3-4 times and dried in a constant temperature drying oven at 50°C to obtain intermediate 3. The ratio of cyanuric chloride, toluene, intermediate 2, and sodium hydroxide solution is 19.1g:150mL:54.7g:50mL.

[0023] Cyanuric chloride reacts with intermediate 2, and sodium hydroxide solution is used as an acid binding agent to promote the reaction to obtain intermediate 3. The specific reaction process is as follows:

[0024]

[0025] S4, in a four-necked bottle, the intermediate 3 and toluene were mixed and stirred evenly, and the temperature was gradually increased to 40°C, and then p-phenylenediamine and sodium hydroxide solution (mass fraction 8%) were added to the above reaction system, and the temperature was slowly increased to 100°C. After the reaction was completed after the heat preservation reaction for 15 hours, the reaction was cooled to room temperature, filtered, washed with distilled water and ethanol, and dried in a vacuum drying oven at 65°C to obtain an auxiliary agent; the ratio of the amount of intermediate 3, toluene, p-phenylenediamine, and sodium hydroxide solution was 69.4g:200mL:10.8g:100mL;

[0026] Intermediate 3 reacts with p-phenylenediamine, and sodium hydroxide solution is used as an acid binding agent to promote the reaction to obtain an auxiliary agent. The specific reaction process is as follows:

[0027]

[0028] The auxiliary agent prepared by the present invention is a macromolecule with good migration and exudation resistance and stable performance. The auxiliary agent also contains a triazine structure, a long carbon chain and a benzene ring structure. The triazine compound contains a tertiary nitrogen structural unit, has a good carbon-forming effect, and can play a synergistic role with the P element in the auxiliary agent to greatly enhance the flame retardant and smoke suppression performance of the matrix. In addition, the triazine compound has a high nitrogen content and releases non-combustible gases such as ammonia during thermal degradation, and also has the function of a foaming agent, without the need to add an additional foaming agent, thereby ensuring the homogeneity of the matrix. The introduced long carbon chain is a methylene chain segment, which is a flexible chain segment, which can not only improve the flexibility of the matrix and thus enhance the impact resistance, but also be interspersed in the macromolecular chain of the matrix to further improve the stability of the auxiliary agent. The introduced benzene ring not only improves the mechanical strength of the matrix to a certain extent, but also improves the compatibility between the auxiliary agent and the matrix, so that the performance of the auxiliary agent is fully exerted.

[0029] Beneficial effects of the present invention:

[0030] 1. The foamed material prepared by the present invention uses polystyrene as a matrix, which gives the material light weight and heat preservation properties;

[0031] 2. Blending SBS with polystyrene can improve the impact resistance of foaming materials;

[0032] 3. By modifying nano-silica, it has better compatibility with the polystyrene matrix than ordinary nano-silica, which can not only improve the mechanical strength of the foaming material, but also serve as a nucleating agent, making the pore size smaller, the pores more numerous, the distribution more uniform, and the performance better;

[0033] 4. The prepared additive is a macromolecule, which not only acts as a foaming agent, but also the various groups in the additive can play a synergistic role, significantly improving the flame retardancy, smoke suppression and impact resistance of the material, and the performance is long-lasting and stable and not easy to fall off;

[0034] Therefore, the foamed material prepared by the present invention is light in weight, has good thermal insulation performance, small pore size, excellent performance, and also has stable and efficient flame retardancy, smoke suppression and impact resistance, and has important application value in the field of foamed material technology. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Embodiment 1

[0037] Preparation aids:

[0038] S1. In a three-necked flask equipped with a stirring device, 11.4 g of diethylenetriamine, 28.4 g of stearic acid and 150 mL of toluene were mixed and stirred evenly, 20.6 g of dicyclohexylcarbodiimide was added, the device was placed in a water bath, and the reaction was kept at 50° C. for 3 h. After the reaction was completed, the mixture was filtered, the solvent was removed by rotary evaporation, the mixture was washed twice with anhydrous ethanol, and the mixture was dried in vacuo to obtain intermediate 1;

[0039] S2, in a three-necked flask equipped with a stirring device, add 36.9g of intermediate 1, 19.6g of diethylphosphoacetic acid, 20.6g of dicyclohexylcarbodiimide and 150mL of toluene, stir and mix well, place in a 55°C water bath, heat in a water bath for 6h, filter after the reaction, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 5:1), and remove the eluent by rotary evaporation to obtain intermediate 2;

[0040] S3, in a three-necked flask, 19.1g of cyanuric chloride and 150mL of toluene were stirred and mixed evenly under an ice bath, and then 54.7g of intermediate 2 was added to the reaction system, and 50mL of sodium hydroxide solution (mass fraction 4%) was slowly added dropwise, and the reaction was carried out while dropping, and the reaction temperature was controlled at 0°C. After the dropwise addition was completed, the reaction was continued for 2h. After the reaction was completed, it was filtered, and the solvent was removed by distillation under reduced pressure, washed with chloroform 3 times, and dried in a constant temperature drying oven at 50°C to obtain intermediate 3;

[0041] S4. Mix 69.4 g of intermediate 3 and 200 mL of toluene in a four-necked bottle and stir evenly, and gradually increase the temperature to 40°C. Then add 10.8 g of p-phenylenediamine and 100 mL of sodium hydroxide solution (mass fraction 8%) to the above reaction system, and slowly increase the temperature to 100°C. After the reaction is kept warm for 15 hours, the reaction is completed. The mixture is cooled to room temperature, filtered, washed thoroughly with distilled water and ethanol, and dried in a vacuum drying oven at 65°C to obtain an auxiliary agent.

[0042] Embodiment 2

[0043] Preparation aids:

[0044] S1. In a three-necked flask equipped with a stirring device, 22.8 g of diethylenetriamine, 56.8 g of stearic acid and 300 mL of toluene were mixed and stirred evenly, 41.2 g of dicyclohexylcarbodiimide was added, and the device was placed in a water bath, and the reaction was kept at 50° C. for 3 h. After the reaction was completed, the mixture was filtered, the solvent was removed by rotary evaporation, the mixture was washed twice with anhydrous ethanol, and the mixture was dried in vacuo to obtain intermediate 1;

[0045] S2, in a three-necked flask equipped with a stirring device, add 73.8g of intermediate 1, 39.2g of diethylphosphoacetic acid, 41.2g of dicyclohexylcarbodiimide and 300mL of toluene, stir and mix well, place in a 55°C water bath, heat in a water bath for 6h, filter after the reaction, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 5:1), and remove the eluent by rotary evaporation to obtain intermediate 2;

[0046] S3, in a three-necked flask, 38.2g of cyanuric chloride and 300mL of toluene were stirred and mixed evenly under an ice bath, and then 109.4g of intermediate 2 was added to the reaction system, and 100mL of sodium hydroxide solution (mass fraction 4%) was slowly added dropwise, and the reaction was carried out while dropping, and the reaction temperature was controlled at 0°C. After the dropwise addition was completed, the reaction was continued for 2h. After the reaction was completed, it was filtered, and the solvent was removed by distillation under reduced pressure, washed with chloroform 3 times, and dried in a constant temperature drying oven at 50°C to obtain intermediate 3;

[0047] S4. In a four-necked bottle, 138.8 g of intermediate 3 and 400 mL of toluene were mixed and stirred evenly, and the temperature was gradually increased to 40°C. Then, 21.6 g of p-phenylenediamine and 200 mL of sodium hydroxide solution (mass fraction 8%) were added to the above reaction system, and the temperature was slowly increased to 100°C. After the reaction was kept warm for 15 hours, the reaction was completed, and the mixture was cooled to room temperature, filtered, washed thoroughly with distilled water and ethanol, and dried in a vacuum drying oven at 65°C to obtain an auxiliary agent.

[0048] Embodiment 3

[0049] Preparation of modified nano-silica:

[0050] Mix 1.0 g of nano-silica with 100 mL of ethanol-water solution, add to a magnetic stirring device, add a magnet, start stirring, and disperse for 35 minutes to evenly disperse the nano-silica in the ethanol-water solution. Evacuate the device, introduce N2 gas, add 6.5 g of γ-glycidyloxypropyltrimethoxysilane, control the temperature to 80°C, and keep the reaction for 4 hours. After the reaction is completed, filter, wash with ethanol, and dry in a vacuum drying oven for 2 hours to obtain modified nano-silica.

[0051] Embodiment 4

[0052] Preparation of modified nano-silica:

[0053] Mix 2.0 g of nano-silica with 200 mL of ethanol-water solution, add them to a magnetic stirring device, add a magnet, start stirring, and disperse for 35 minutes to evenly disperse the nano-silica in the ethanol-water solution. Evacuate the device, introduce N2 gas, and then add 13.0 g of γ-glycidyloxypropyltrimethoxysilane. Control the temperature to 80°C and keep the reaction warm for 4 hours. After the reaction is completed, filter, wash with ethanol, and dry in a vacuum drying oven for 2 hours to obtain modified nano-silica.

[0054] Embodiment 5

[0055] 60g of polystyrene, 10g of styrene-butadiene-styrene, 4g of the modified nano-silica prepared in Example 3, 5g of the auxiliary agent prepared in Example 1 and 3g of paraffin were mixed, added to a twin-screw extruder, melt blended, extruded, and injected into an expansion extruder for foaming. After foaming, a flame-retardant polymer foam material was obtained.

[0056] Embodiment 6

[0057] 70g of polystyrene, 15g of styrene-butadiene-styrene, 6g of the modified nano-silica prepared in Example 3, 10g of the auxiliary agent prepared in Example 2 and 4g of stearamide fatty acid were mixed, added to a twin-screw extruder, melt blended, extruded, and injected into an expansion extruder for foaming. After foaming, a flame-retardant polymer foam material was obtained.

[0058] Embodiment 7

[0059] 80g of polystyrene, 20g of styrene-butadiene-styrene, 8g of the modified nano-silica prepared in Example 4, 15g of the auxiliary agent prepared in Example 2 and 5g of stearamide fatty acid were mixed, added to a twin-screw extruder, melt blended, extruded, and injected into an expansion extruder for foaming. After foaming, a flame-retardant polymer foam material was obtained.

[0060] Comparative Example 1

[0061] The auxiliary agent in Example 7 was replaced by a commercially available nitrogen-based flame retardant of equal quality, and the remaining steps were the same as those in Example 7 to obtain a foaming material.

[0062] Comparative Example 2

[0063] Commercially available polystyrene foam material was used.

[0064] Embodiments 5, 6, 7 and comparative examples 1 and 2 were made into corresponding shapes according to different test standards and subjected to the following performance tests:

[0065] The national standard GB / T 2406-2008 "Test method for combustion performance of plastics" is used to measure the limiting oxygen index of the sample before and after standing at room temperature for 180 days;

[0066] The national standard GB / T 8323.2-2008 "Plastic Smoke Generation Part 2: Single Chamber Test Method for Determining Smoke Density" was used to measure the smoke density of the sample before and after standing at room temperature for 180 days;

[0067] The notched impact strength is measured using the national standard GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics";

[0068] The measured results are shown in the following table:

[0069]

[0070]

[0071] It can be seen from the above table that the foam material prepared in the embodiment of the present invention has higher flame retardancy, smoke suppression and impact resistance than the control example, and the performance is long-lasting and stable, which has important application value in the field of foam material technology.

[0072] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0073] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a flame retardant polymer foam material, characterized in that: The following steps are involved: Polystyrene, styrene-butadiene-styrene, modified nano-silica, additives and lubricants are mixed, added into a twin-screw extruder, melt-blended, extruded, and then injected into an expansion extruder for foaming to obtain a flame-retardant polymer foam material.

2. The method for preparing a flame retardant polymer foam material according to claim 1, characterized in that: The auxiliary agent is prepared by the following steps: S1. Mix diethylenetriamine, stearic acid and toluene and stir evenly, add dicyclohexylcarbodiimide, place in a water bath, react at 50°C for 3h, filter, rotary evaporate, wash and dry to obtain intermediate 1; S2, mixing intermediate 1, diethylphosphoacetic acid, dicyclohexylcarbodiimide and toluene, placing in a water bath, heating at 55°C for 6 h, filtering, vacuum distilling, column chromatography purification, rotary evaporation to obtain intermediate 2; S3, after cyanuric chloride and toluene are stirred and mixed evenly in an ice bath, intermediate 2 is added to the reaction system, and sodium hydroxide solution is slowly added dropwise, and the reaction is carried out while dropping, and the reaction temperature is controlled at 0°C. After the dropwise addition is completed, the reaction is continued for 2 hours. After the reaction is completed, the reaction is filtered, distilled under reduced pressure, washed, and dried to obtain intermediate 3; S4. Mix the intermediate 3 and toluene and stir evenly, and gradually increase the temperature to 40°C, then add p-phenylenediamine and sodium hydroxide solution, and slowly increase the temperature to 100°C. After keeping the reaction for 15 hours, the reaction is completed, and the mixture is cooled to room temperature, filtered, washed, and dried to obtain an auxiliary agent.

3. The method for preparing a flame retardant polymer foam material according to claim 2, characterized in that: In step S1, the ratio of diethylenetriamine, stearic acid, toluene and dicyclohexylcarbodiimide is 11.4 g: 28.4 g: 150 mL: 20.6 g.

4. The method for preparing a flame retardant polymer foam material according to claim 2, characterized in that: In step S2, the ratio of the amount of intermediate 1, diethylphosphoacetic acid, dicyclohexylcarbodiimide and toluene is 36.9 g:19.6 g:20.6 g:150 mL.

5. The method for preparing a flame retardant polymer foam material according to claim 2, characterized in that: In step S3, the ratio of cyanuric chloride, toluene, intermediate 2, and sodium hydroxide solution is 19.1 g: 150 mL: 54.7 g: 50 mL.

6. The method for preparing a flame retardant polymer foam material according to claim 2, characterized in that: In step S4, the ratio of the amount of intermediate 3, toluene, p-phenylenediamine, and sodium hydroxide solution is 69.4 g: 200 mL: 10.8 g: 100 mL.

7. The method for preparing a flame-retardant polymer foam material according to claim 1, characterized in that: The raw materials are calculated in parts by weight as follows: 60-80 parts of polystyrene, 10-20 parts of styrene-butadiene-styrene, 4-8 parts of modified nano silicon dioxide, 5-15 parts of auxiliary agent, and 3-5 parts of lubricant.

8. The method for preparing a flame retardant polymer foam material according to claim 1, characterized in that: The modified nano silicon dioxide is prepared by the following steps: The nano-silica was mixed with an ethanol aqueous solution, magnetically stirred, dispersed for 35 minutes, the device was evacuated, N2 gas was introduced, and γ-glycidyloxypropyltrimethoxysilane was added. The mixture was reacted at 80°C for 4 hours. After the reaction was completed, the mixture was filtered, washed, and dried to obtain modified nano-silica.

9. The method for preparing a flame retardant polymer foam material according to claim 8, characterized in that: The usage ratio of the nano-silica, the ethanol aqueous solution and γ-glycidyloxypropyltrimethoxysilane is 1.0 g:100 mL:6.5 g.

10. A flame retardant polymer foam material, characterized in that: Prepared according to the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Protective coating for limiting rope in aviation oxygen supply mask pipeline and preparation method of protective coating

    CN120005464A

  • A protective coating for the restraining cord inside the air supply mask pipeline of an aircraft and its preparation method

    CN120005464B

  • Silicone rubber thermal insulation material for heater and preparation method of silicone rubber thermal insulation material

    CN120648246A