Method for preparing flame-retardant heat-insulation pad from PBO waste filament chopped fibers

By mixing the phosphorus-based flame-retardant polymer with aerogel and dispersing additive with short-cut fibers of PBO waste silk, the flame-retardant heat insulation pad was prepared, which solved the problem of waste silk utilization in PBO fiber production, and achieved efficient improvement in the addition of waste silk The preparation of thermal insulation pads with excellent value and performance has broadened the application field.

CN119060480APending Publication Date: 2024-12-03SHANDONG NON METALLIC MATERIAL RESEARCH INSTITUTE
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411266036.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The waste silk produced during PBO fiber production is difficult to effectively utilize, resulting in high production costs and single products, and lack of diversity.

Method used

The phosphorus-based flame retardant polymer was mixed with aerogel and dispersion additive, and chopped PBO waste wire fibers were added, and the flame retardant heat insulation pad was prepared after drying and pressurizing.

Benefits of technology

The added value of PBO waste wire is improved, and the flame-retardant heat insulation pad with excellent performance is prepared, which has good fire-proof and heat-resistant properties and heat resistance, which broadens the application field of PBO fiber and realizes the efficient utilization of waste wire.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of application of high-performance fibers, and particularly relates to a method for preparing a flame-retardant heat-insulation pad from PBO waste filament chopped fibers. The flame-retardant heat insulation mat is composed of PBO waste filament chopped fibers, phosphorus flame-retardant polymers and a small amount of aerogel, the tensile strength of the flame-retardant heat insulation mat can reach 6500 MPa, the limit oxygen index reaches 53%, and the heat conductivity coefficient is as low as 0.021 w / m.k. The preparation method comprises the following specific preparation steps: firstly, adding water to dissolve the phosphorus flame-retardant polymer, then adding the aerogel and the dispersing aid, uniformly dispersing to obtain a dispersion liquid capable of being used as a filler, finally, putting a certain part of PBO waste filament chopped fiber into the dispersion liquid, fully dispersing, and then drying and calendering to obtain the flame-retardant heat-insulating pad. The preparation method has the characteristics that the PBO waste filament chopped fiber is taken as a main component, the additional value of the PBO waste filament can be efficiently improved, the production cost of the PBO fiber can be reduced, and the prepared flame-retardant heat-insulation pad has excellent fireproof heat-insulation performance and can be self-extinguished when being away from fire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-performance fiber applications, and in particular relates to a method for preparing a flame-retardant heat-insulating pad from PBO waste chopped fibers. Background Art

[0002] Poly(p-phenylene benzobisoxazole) (PBO) fiber is currently the most excellent organic reinforcing fiber material with comprehensive performance. Due to its high modulus, high strength, good flame retardancy and high temperature resistance and many other excellent properties, it is widely used in lightweight composite materials, bulletproof vests, armor protection and thermal protection, and has broad application prospects in the aerospace field. In the late 1990s, Japan's Toyobo Co., Ltd. announced that it had obtained high-performance PBO fiber, trade name Zylon, and applied Zylon to high-tech fields such as aerospace and national defense.

[0003] At present, in the production of PBO fiber, especially in the spinning process, a certain amount of PBO waste fibers will inevitably be produced. The comprehensive utilization of these waste fibers to reduce the production cost of PBO fiber has become an urgent problem that all PBO fiber manufacturers need to solve. Cutting the PBO fiber waste fibers with a fiber cutting machine and then preparing the PBO waste fibers into flame-retardant insulation mats through a series of technical means can expand the application field of PBO fiber and increase the diversity of its products. Summary of the invention

[0004] In view of the existing problems, the present invention provides a method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers. The method dissolves a phosphorus-based flame retardant polymer in water, then adds aerogel and a dispersing aid and disperses them evenly to obtain a dispersion liquid that can be used as a filler. Finally, a certain number of PBO waste chopped fibers are placed in the dispersion liquid and fully dispersed, and then dried and pressed to obtain a flame retardant thermal insulation pad. With PBO waste chopped fibers as the main component, the problem of single PBO fiber products and waste fiber utilization in the spinning process is solved, and the added value of PBO waste fibers can be efficiently improved to prepare flame retardant thermal insulation pads with excellent performance.

[0005] Furthermore, the specific technical solution of the present invention is:

[0006] A method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers, specifically comprising the following steps:

[0007] (1) adding water to a phosphorus-based flame-retardant polymer and stirring and dissolving the polymer to obtain a colorless and transparent flame-retardant polymer solution;

[0008] (2) adding aerogel and a dispersing aid into the flame retardant polymer solution and continuing stirring to obtain a dispersion liquid that can be used as a filler for a flame retardant thermal insulation pad;

[0009] (3) After the PBO waste chopped fibers are fully dispersed in a dispersion liquid, they are pre-dried, pressed, and dried at high temperature to obtain a flame retardant thermal insulation mat.

[0010] Preferably, the phosphorus-based flame retardant polymer in step (1) is selected from the esterification product of polyvinyl alcohol and a phosphorus-based flame retardant containing a phosphoric acid group.

[0011] Preferably, in step (1), the phosphorus-based flame-retardant polymer is dissolved by stirring in a water bath, the water bath temperature is 40 to 60° C., and the stirring time is 6 to 8 hours.

[0012] The phosphorus-based flame retardant containing a phosphoric acid group can be any existing technology, but in order to obtain better effects, it is preferably inositol hexaphosphate, pyrophosphate, acetyl phosphate, 1,3-diphosphoglyceric acid, phosphoenolpyruvic acid, creatine phosphate, etc.

[0013] Preferably, the aerogel described in step (2) is one of Si3N4 aerogel, BN aerogel or SiO2, TiO2, Al2O3 aerogel.

[0014] Preferably, the dispersing aid described in step (2) is one or a combination of two of polyethylene oxide (PEO), cetyltrimethylammonium bromide (CTAB), vinyl bisstearamide (EBS), stearic acid monoglyceride (GMS), and tristearin (HTG).

[0015] More preferably, the stirring time in step (2) is 6 to 8 hours.

[0016] Preferably, in the flame retardant thermal insulation pad, the addition ratio between the flame retardant polymer and the PBO waste chopped fibers is 1 to 2:1, and the addition ratio between the aerogel and the PBO waste chopped fibers is 0.2 to 1:1.

[0017] Preferably, in the flame retardant thermal insulation pad, the amount of the dispersing aid is 5% to 15% (mass percentage) of the amount of PBO waste chopped fibers added.

[0018] Preferably, the length of the PBO waste chopped fibers in step (3) is 0.5 to 4 mm.

[0019] More preferably, the dispersion time in step (3) is 4 to 6 hours.

[0020] More preferably, the pre-drying temperature in step (3) is 60-80°C, the pre-drying time is 3-5 hours, and the high-temperature drying temperature is 140-160°C, and the time is 1-2 hours.

[0021] The beneficial effects of the present invention are:

[0022] PBO waste silk is a product whose mechanical properties do not meet the filament use standards due to various reasons during the production process of PBO fibers, but its thermal properties are still relatively excellent. The present invention uses PBO waste silk chopped fibers as the main component to prepare a flame-retardant thermal insulation pad, and uses phosphorus-based flame-retardant polymers and aerogels as fillers for the thermal insulation pad, supplemented by a better preparation method, so that the PBO waste silk chopped fibers are evenly distributed inside, which can give full play to its high flame retardant and high heat-resistant properties. The prepared flame-retardant thermal insulation pad is smooth and flat, and has excellent flame retardant and heat-resistant properties; it solves the problem of single PBO fiber products and the use of waste silk in the spinning process, and can efficiently increase the added value of PBO waste silk and improve its economic benefits. In summary, the flame-retardant thermal insulation pad prepared by the method of the present invention has excellent fireproof and heat-insulating properties, and can achieve self-extinguishing from fire. At the same time, it broadens the application field of PBO waste silk, turning waste into treasure, saving resources and increasing efficiency. DETAILED DESCRIPTION

[0023] The above contents of the present invention are further described in detail below by means of specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Unless otherwise specified, conventional technical operations are used in the following embodiments.

[0024] Example 1

[0025] A method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers comprises the following steps:

[0026] (1) 80 g of a phosphorus-based flame-retardant polymer obtained by esterification of polyvinyl alcohol and inositol hexaphosphate was added to 400 ml of water in a 70° C. water bath and stirred for 7 h to obtain a flame-retardant polymer solution.

[0027] (2) Add 20 g of Si3N4 aerogel and 5 g of polyethylene oxide to the above solution, stir and mix thoroughly to obtain a dispersion liquid that can be used as a filler for flame retardant thermal insulation pads.

[0028] (3) 40 g of PBO waste chopped fibers (fiber length of about 1 mm) were added to the above dispersion and dispersed for 4 h. The solution was then pre-dried at 60° C. for 3 h to obtain a colloid having adhesiveness and tensile ductility.

[0029] (4) The colloid is heated and pressed by a calendering machine to obtain a flame retardant thermal insulation pad with a smooth surface and regular size, and finally the flame retardant thermal insulation pad is dried at a high temperature of 150°C to obtain a finished flame retardant thermal insulation pad. The obtained flame retardant thermal insulation pad has a tensile strength of 5300 MPa, a limiting oxygen index of 49%, and a thermal conductivity as low as 0.029 w / m˙k.

[0030] Example 2

[0031] A method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers comprises the following steps:

[0032] (1) 80 g of a phosphorus-based flame-retardant polymer obtained by esterification of polyvinyl alcohol and inositol hexaphosphate was added to 400 ml of water at 70° C. and stirred for 7 hours to obtain a flame-retardant polymer solution.

[0033] (2) Add 20 g of TiO2 aerogel and 5 g of hexadecyltrimethylammonium bromide to the above solution, stir and mix thoroughly to obtain a dispersion liquid that can be used as a filler for flame retardant thermal insulation pads.

[0034] (3) 60 g of PBO waste chopped fibers (fiber length of about 3 mm) were added to the above dispersion and dispersed for 4 h. The solution was then pre-dried at 60° C. for 3 h to obtain a colloid having adhesiveness and tensile ductility.

[0035] (4) The colloid is heated and pressed by a calendering machine to obtain a flame retardant thermal insulation pad with a smooth surface and regular size, and finally the flame retardant thermal insulation pad is dried at a high temperature of 150°C to obtain a finished flame retardant thermal insulation pad. The obtained flame retardant thermal insulation pad has a tensile strength of 6100 MPa, a limiting oxygen index of 52%, and a thermal conductivity as low as 0.026 w / m˙k.

[0036] Example 3

[0037] (1) 80 g of a phosphorus-based flame-retardant polymer obtained by esterifying polyvinyl alcohol with creatine phosphate was added to 400 ml of water at 70° C. and stirred for 7 h to obtain a flame-retardant polymer solution.

[0038] (2) Add 20 g of SiO2 aerogel and 5 g of polyethylene oxide to the above solution, stir and mix thoroughly to obtain a dispersion liquid that can be used as a filler for flame retardant thermal insulation pads.

[0039] (3) 80 g of PBO waste chopped fibers (fiber length of about 3 mm) were added to the above dispersion and dispersed for 4 h. The solution was then pre-dried at 60° C. for 3 h to obtain a colloid having adhesiveness and tensile ductility.

[0040] (4) The colloid is heated and pressed into shape by a calendering machine to obtain a flame retardant thermal insulation pad with a smooth surface and regular size, and finally the flame retardant thermal insulation pad is dried at a high temperature of 150°C to obtain a finished flame retardant thermal insulation pad. The obtained flame retardant thermal insulation pad has a tensile strength of 6500MPa, a limiting oxygen index of 53%, and a thermal conductivity as low as 0.021w / m˙k.

[0041] Comparative Example 1

[0042] (1) A phosphorus-based flame-retardant polymer obtained by esterification reaction of 80 g of polyvinyl alcohol and inositol hexaphosphate was added to 400 ml of water at 70° C. and stirred for 7 hours to obtain a flame-retardant polymer solution.

[0043] (2) Add 20 g of SiO2 aerogel and 5 g of polyethylene oxide to the above solution, stir and mix thoroughly to obtain a dispersion liquid that can be used as a filler for flame retardant thermal insulation pads.

[0044] (3) Add 80 g of aramid chopped fibers (fiber length of about 3 mm) to the above dispersion and disperse for 10 h. Then pre-dry the solution at 60° C. for 3 h to obtain a colloid having adhesiveness and tensile ductility.

[0045] (4) The colloid is heated and pressed by a calendering machine to obtain a flame retardant thermal insulation pad with a smooth surface and regular size, and finally the flame retardant thermal insulation pad is dried at a high temperature of 150°C to obtain a finished flame retardant thermal insulation pad. The obtained flame retardant thermal insulation pad has a tensile strength of 4300 MPa, a limiting oxygen index of 29%, and a thermal conductivity of 0.039 w / m˙k.

[0046] The chopped fibers used in Comparative Example 1 are aramid chopped fibers. Although flame retardant thermal insulation pads can also be prepared by the same process route as Examples 1-3, the performance of the flame retardant thermal insulation pads in the comparative example is far lower than that of the present invention, especially the limiting oxygen index of the flame retardant thermal insulation pads in the comparative example is only 29%, which only reaches the level of flame retardancy. This shows that although the present invention uses PBO waste chopped fibers as raw materials, high-quality flame retardant thermal insulation pads can be obtained through the method of the present invention, which broadens the application field of PBO fibers and greatly improves the economic benefits of PBO fiber production enterprises.

Claims

1. A method for preparing a flame retardant thermal insulation mat from PBO waste chopped fibers, comprising the following steps: (1) adding water to a phosphorus-based flame-retardant polymer in a water bath at a certain temperature and stirring to dissolve the polymer to obtain a colorless and transparent flame-retardant polymer solution; (2) adding aerogel and a dispersing aid into the flame retardant polymer solution and continuing stirring to obtain a dispersion liquid that can be used as a filler for a flame retardant thermal insulation pad; (3) After a certain amount of PBO waste chopped fibers are fully dispersed in a dispersion liquid, a flame retardant thermal insulation mat is obtained through pre-drying, calendering and high-temperature drying.

2. According to claim 1, a method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers, It is characterized in that In step (1), the phosphorus-based flame retardant polymer is an esterification product of polyvinyl alcohol and a phosphorus-based flame retardant containing a phosphoric acid group, the water bath temperature is 40-60° C., and the stirring time is 6-8 hours.

3. According to claim 1, a method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers, It is characterized in that In step (2), the aerogel is Si 3 N 4 Aerogel, BN aerogel or SiO 2 、TiO 2 、Al 2 O 3 A type of aerogel.

4. According to claim 1, a method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers, It is characterized in that The dispersing aid in step (2) is one or a combination of two of polyethylene oxide (PEO), cetyltrimethylammonium bromide (CTAB), vinyl bisstearamide (EBS), stearic acid monoglyceride (GMS), and tristearin (HTG).

5. According to claim 1, a method for preparing a flame retardant thermal insulation pad from PBO waste chopped fibers, It is characterized in that The stirring time in step (2) is 6 to 8 hours.

6. A method for preparing a flame retardant thermal insulation mat from PBO waste chopped fibers according to claim 1, It is characterized in that The addition ratio of the flame retardant polymer to the PBO waste chopped fibers is 1 to 2:1, and the addition ratio of the aerogel to the PBO waste chopped fibers is 0.2 to 1:

1.

7. A method for preparing a flame retardant thermal insulation mat from PBO waste chopped fibers according to claim 1, It is characterized in that The amount of the dispersing aid is 5% to 15% of the amount of the PBO waste chopped fibers added.

8. According to claim 1, a method for preparing a flame retardant thermal insulation mat from PBO waste chopped fibers, It is characterized in that In step (3), the length of the chopped PBO waste fibers is 0.5 to 4 mm.

9. A method for preparing a flame retardant thermal insulation mat from PBO waste chopped fibers according to claim 1, It is characterized in that The dispersion time in step (3) is 4 to 6 hours.

10. A method for preparing a flame retardant thermal insulation mat from PBO waste chopped fibers according to claim 1, It is characterized in that In step (3), the pre-drying temperature is 60-80° C., the pre-drying time is 3-5 h, and the high-temperature drying temperature is 140-160° C., and the time is 1-2 h.

Citation Information

Cited By

  • Boron modified polybenzoxazole fiber aerogel and preparation method thereof

    CN119639074A

  • Nano-alumina modified polybenzoxazole fiber aerogel and preparation method thereof

    CN119639075A

  • A nano-alumina modified polybenzoxazole fiber aerogel and preparation method thereof

    CN119639075B