Optical lens capable of shielding harmful light and correcting vision and preparation method thereof

By using epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorbers and CR39 resin in optical lenses, combined with wavefront aberration calculation technology, the damage problem of harmful light emitted by electronic products to the eyes is solved, and the damage problem of harmful light emitted by electronic products is achieved. Excellent shielding effect and vision correction have been used to significantly improve the overall performance of the lens.

CN119060482APending Publication Date: 2024-12-03XINSHIJIE HEALTH TECH (JILIN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115297.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Long-term exposure to harmful light emitted by electronic products can lead to eye pressure, red eyes, dry eyes, decreased vision and eye diseases. The prior art is difficult to effectively block harmful light and correct vision.

Method used

Optical lenses are prepared through specific ratios and process processing using a combination of epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorbers and CR39 resin monomers, combining wavefront aberration calculation technology and advanced aberration elimination technology Design optical curvature to achieve corrective vision.

Benefits of technology

The prepared optical lens has excellent anti-blue light and ultraviolet ray functions, while improving mechanical properties and light transmittance, significantly improving overall performance, and effectively protecting vision health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993455200000091
    Figure BDA0004993455200000091
Patent Text Reader

Abstract

The invention discloses an optical lens capable of shielding harmful light and correcting vision and a preparation method of the optical lens. The optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage by weight: 3%-5% of epoxy resin, 0.5%-1.2% of nano iron oxide, 0.5%-1% of carbon nanotubes, 1%-4% of an ultraviolet light absorber, 1%-1.5% of an initiator and the balance of CR39 resin monomers. The preparation raw materials and dosage are limited, so that the prepared optical lens capable of shielding harmful light and correcting vision has an excellent function of shielding harmful light and also has excellent mechanical properties and light transmittance, specifically, epoxy resin is added for modification, so that the light transmittance and mechanical properties of the material can be improved, and the optical lens can be used for correcting vision. According to the optical lens, harmful light can be better shielded by adding the carbon nanotubes, the nano iron oxide and the ultraviolet light absorber, meanwhile, the mechanical property of the material is improved, and in addition, the purpose of correcting vision can be achieved through curvature setting of the optical lens.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical materials, and in particular to an optical lens capable of shielding harmful light and correcting vision and a preparation method thereof. Background Art

[0002] LED lights, TVs, computer monitors, smart phones, tablets and other products are now widely used in all aspects of people's lives. The light emitted by these products contains a large amount of irregular frequency high-energy short-wave blue light. Watching images, texts, videos, etc. at close range for a long time will cause certain pressure on the eyes, resulting in symptoms such as red eyes, dry eyes, astringent eyes, blurred vision, visual fatigue, and pain in the head, back, shoulders and cervical spine.

[0003] With the popularity of electronic products and people's habit of facing electronic screens for a long time, harmful light is increasingly harmful to the eyes. Harmful light not only causes vision loss, but may also cause eye diseases. Therefore, developing an optical lens that can shield harmful light and correct vision is of great significance to protecting people's vision health.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide an optical lens capable of shielding harmful light and correcting vision and a method for preparing the same. The optical lens of the present invention has excellent blue light protection and UV resistance functions, as well as excellent mechanical properties and light transmittance.

[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0007] The first aspect of the present invention provides an optical lens capable of shielding harmful light and correcting vision, wherein the optical lens capable of shielding harmful light and correcting vision comprises raw materials in the following percentages:

[0008] Epoxy resin 3%-5%, nano iron oxide 0.5%-1.2%, carbon nanotube 0.5%-1%, ultraviolet absorber 1%-4%, initiator 1%-1.5%, and the balance is CR39 resin monomer.

[0009] Preferably, the optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage:

[0010] Epoxy resin 3.5%-4.5%, nano iron oxide 0.8%-1.0%, carbon nanotube 0.6%-0.8%, ultraviolet absorber 2%-3%, initiator 1.2%-1.5%, and the balance is CR39 resin monomer.

[0011] Preferably, the optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage:

[0012] Epoxy resin 4%, nano iron oxide 1%, carbon nanotubes 0.8%, ultraviolet absorber 3%, initiator 1.2%, and the balance is CR39 resin monomer.

[0013] Preferably, the ultraviolet absorber is selected from at least one of UV-P, UV-327, UV-360 and UV-928.

[0014] Preferably, the initiator is diisopropyl peroxydicarbonate.

[0015] The second aspect of the present invention provides a method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision, the preparation method comprising the following steps:

[0016] (a) weighing each raw material according to weight;

[0017] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0018] (c) adding an initiator to the mixture for heating reaction to obtain a reactant;

[0019] (d) adding the reactants into a mold for heating and curing, demolding, and continuing heating for secondary curing to obtain the optical lens capable of shielding harmful light and correcting vision.

[0020] Preferably, in step (c), the heating reaction temperature is 50-60° C. and the reaction time is 2-3 h.

[0021] Preferably, in step (d), the heating and curing is performed by raising the temperature to 85° C. within 16 to 18 hours.

[0022] Preferably, in the step (d), the secondary curing temperature is 125-130° C. and the time is 2-3 hours.

[0023] Compared with the prior art, the beneficial effects of the present invention include at least:

[0024] The present invention limits the preparation raw materials and dosage, so that the prepared optical lens capable of shielding harmful light and correcting vision has excellent function of shielding harmful light, and at the same time has excellent mechanical properties and light transmittance. Specifically, by adding epoxy resin for modification, the light transmittance and mechanical properties of the material can be improved. The addition of carbon nanotubes, nano-iron oxide and ultraviolet absorbers can achieve better shielding of harmful light and improve the mechanical properties of the material. Through the reasonable proportion of the raw materials, the overall performance of the prepared optical lens is significantly improved.

[0025] In addition, the optical lens for shielding harmful light and correcting vision of the present invention can be designed with corresponding optical curvature through wavefront aberration calculation technology and high-order aberration elimination technology, so as to achieve correction of vision. DETAILED DESCRIPTION

[0026] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.

[0027] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the invention belongs.

[0028] The first aspect of the present invention provides an optical lens capable of shielding harmful light and correcting vision, wherein the optical lens capable of shielding harmful light and correcting vision comprises raw materials in the following percentages:

[0029] Epoxy resin 3%-5%, nano iron oxide 0.5%-1.2%, carbon nanotube 0.5%-1%, ultraviolet absorber 1%-4%, initiator 1%-1.5%, and the balance is CR39 resin monomer.

[0030] The present invention limits the preparation raw materials and dosage, so that the prepared optical lens capable of shielding harmful light and correcting vision has excellent function of shielding harmful light, and at the same time has excellent mechanical properties and light transmittance. Specifically, by adding epoxy resin for modification, the light transmittance and mechanical properties of the material can be improved. The addition of carbon nanotubes, nano-iron oxide and ultraviolet absorbers can achieve better shielding of harmful light and improve the mechanical properties of the material. Through the reasonable proportion of the raw materials, the overall performance of the prepared optical lens is significantly improved.

[0031] In one embodiment, the optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage:

[0032] Epoxy resin 3.5%-4.5%, nano iron oxide 0.8%-1.0%, carbon nanotube 0.6%-0.8%, ultraviolet absorber 2%-3%, initiator 1.2%-1.5%, and the balance is CR39 resin monomer.

[0033] In one embodiment, the optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage:

[0034] Epoxy resin 4%, nano iron oxide 1%, carbon nanotubes 0.8%, ultraviolet absorber 3%, initiator 1.2%, and the balance is CR39 resin monomer.

[0035] In one embodiment, the ultraviolet absorber is selected from at least one of UV-P, UV-327, UV-360 and UV-928.

[0036] In one embodiment, the initiator is diisopropyl peroxydicarbonate.

[0037] Another embodiment of the present invention provides a method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision, the preparation method comprising the following steps:

[0038] (a) weighing each raw material according to weight;

[0039] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0040] (c) adding an initiator to the mixture for heating reaction to obtain a reactant;

[0041] (d) adding the reactants into a mold for heating and curing, demolding, and continuing heating for secondary curing to obtain the optical lens capable of shielding harmful light and correcting vision.

[0042] In one embodiment, in the step (c), the heating reaction temperature is 50-60° C., and the reaction time is 2-3 hours.

[0043] In one embodiment, in the step (d), the heating curing is to raise the temperature to 85° C. within 16 to 18 hours.

[0044] In one embodiment, in the step (d), the secondary curing temperature is 125-130° C. and the time is 2-3 hours.

[0045] The technical solution of the present invention is further described in detail below through specific embodiments.

[0046] Example 1

[0047] This embodiment is an optical lens capable of shielding harmful light and correcting vision. The optical lens capable of shielding harmful light and correcting vision comprises raw materials with the following percentages:

[0048] Epoxy resin 3%, nano iron oxide 1.2%, carbon nanotubes 0.5%, ultraviolet absorber 1%, initiator 1.5%, the balance is CR39 resin monomer;

[0049] The ultraviolet absorber is UV-360;

[0050] The initiator is diisopropyl peroxydicarbonate.

[0051] The method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision comprises the following steps:

[0052] (a) weighing each raw material according to weight;

[0053] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0054] (c) adding an initiator to the mixture for heating reaction to obtain a reactant, wherein the heating reaction temperature is 50° C. and the reaction time is 3 h;

[0055] (d) adding the reactants into the mold, heating the mold to 85° C. within 16 hours for curing and demolding, and continuing to heat the mold to 125° C. for secondary curing for 3 hours to obtain the optical lens capable of shielding harmful light and correcting vision.

[0056] Example 2

[0057] This embodiment is an optical lens capable of shielding harmful light and correcting vision. The optical lens capable of shielding harmful light and correcting vision comprises raw materials with the following percentages:

[0058] Epoxy resin 5%, nano iron oxide 0.5%, carbon nanotubes 1%, ultraviolet absorber 4%, initiator 1%, the balance is CR39 resin monomer;

[0059] The ultraviolet absorber is UV-360;

[0060] The initiator is diisopropyl peroxydicarbonate.

[0061] The method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision comprises the following steps:

[0062] (a) weighing each raw material according to weight;

[0063] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0064] (c) adding an initiator to the mixture for heating reaction to obtain a reactant, wherein the heating reaction temperature is 60° C. and the reaction time is 2 h;

[0065] (d) adding the reactants into the mold, heating the mold to 85° C. within 18 hours for curing, demolding, and continuing to heat the mold to 130° C. for secondary curing for 2 hours to obtain the optical lens capable of shielding harmful light and correcting vision.

[0066] Example 3

[0067] This embodiment is an optical lens capable of shielding harmful light and correcting vision. The optical lens capable of shielding harmful light and correcting vision comprises raw materials with the following percentages:

[0068] Epoxy resin 3.5%, nano iron oxide 0.8%, carbon nanotubes 0.8%, ultraviolet absorber 2%, initiator 1.2%, the balance is CR39 resin monomer;

[0069] The ultraviolet absorber is UV-360;

[0070] The initiator is diisopropyl peroxydicarbonate.

[0071] The method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision comprises the following steps:

[0072] (a) weighing each raw material according to weight;

[0073] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0074] (c) adding an initiator to the mixture for heating reaction to obtain a reactant, wherein the heating reaction temperature is 55° C. and the reaction time is 2.5 h;

[0075] (d) adding the reactants into the mold, heating the mold to 85° C. within 17 hours for curing and demolding, and then heating the mold to 130° C. for secondary curing for 3 hours to obtain the optical lens capable of shielding harmful light and correcting vision.

[0076] Example 4

[0077] This embodiment is an optical lens capable of shielding harmful light and correcting vision. The optical lens capable of shielding harmful light and correcting vision comprises raw materials with the following percentages:

[0078] Epoxy resin 4.5%, nano iron oxide 1.0%, carbon nanotubes 0.6%, ultraviolet absorber 3%, initiator 1.5%, the balance is CR39 resin monomer;

[0079] The ultraviolet absorber is UV-360;

[0080] The initiator is diisopropyl peroxydicarbonate.

[0081] The method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision comprises the following steps:

[0082] (a) weighing each raw material according to weight;

[0083] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0084] (c) adding an initiator to the mixture for heating reaction to obtain a reactant, wherein the heating reaction temperature is 55° C. and the reaction time is 2.5 h;

[0085] (d) adding the reactants into the mold, heating the mold to 85° C. within 17 hours for curing and demolding, and continuing to heat the mold to 125° C. for secondary curing for 3 hours to obtain the optical lens capable of shielding harmful light and correcting vision.

[0086] Example 5

[0087] This embodiment is an optical lens capable of shielding harmful light and correcting vision. The optical lens capable of shielding harmful light and correcting vision comprises raw materials with the following percentages:

[0088] Epoxy resin 4%, nano iron oxide 1%, carbon nanotubes 0.8%, ultraviolet absorber 3%, initiator 1.2%, the balance is CR39 resin monomer;

[0089] The ultraviolet absorber is UV-360;

[0090] The initiator is diisopropyl peroxydicarbonate.

[0091] The method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision comprises the following steps:

[0092] (a) weighing each raw material according to weight;

[0093] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0094] (c) adding an initiator to the mixture for heating reaction to obtain a reactant, wherein the heating reaction temperature is 55° C. and the reaction time is 2.5 h;

[0095] (d) adding the reactants into the mold, heating the mold to 85° C. within 17 hours for curing and demolding, and then heating the mold to 130° C. for secondary curing for 3 hours to obtain the optical lens capable of shielding harmful light and correcting vision.

[0096] Comparative Example 1

[0097] This comparative example is an optical lens capable of shielding harmful light and correcting vision, and the optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage:

[0098] Nano iron oxide 1%, carbon nanotubes 0.8%, ultraviolet absorber 3%, initiator 1.2%, the balance is CR39 resin monomer;

[0099] The ultraviolet absorber is UV-360;

[0100] The initiator is diisopropyl peroxydicarbonate.

[0101] The method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision comprises the following steps:

[0102] (a) weighing each raw material according to weight;

[0103] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0104] (c) adding an initiator to the mixture for heating reaction to obtain a reactant, wherein the heating reaction temperature is 55° C. and the reaction time is 2.5 h;

[0105] (d) adding the reactants into the mold, heating the mold to 85° C. within 17 hours for curing and demolding, and then heating the mold to 130° C. for secondary curing for 3 hours to obtain the optical lens capable of shielding harmful light and correcting vision.

[0106] Comparative Example 2

[0107] This comparative example is an optical lens capable of shielding harmful light and correcting vision, and the optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage:

[0108] Epoxy resin 4%, nano iron oxide 1%, UV absorber 3%, initiator 1.2%, the balance is CR39 resin monomer;

[0109] The ultraviolet absorber is UV-360;

[0110] The initiator is diisopropyl peroxydicarbonate.

[0111] The method for preparing the above-mentioned optical lens capable of shielding harmful light and correcting vision comprises the following steps:

[0112] (a) weighing each raw material according to weight;

[0113] (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture;

[0114] (c) adding an initiator to the mixture for heating reaction to obtain a reactant, wherein the heating reaction temperature is 55° C. and the reaction time is 2.5 h;

[0115] (d) adding the reactants into the mold, heating the mold to 85° C. within 17 hours for curing and demolding, and then heating the mold to 130° C. for secondary curing for 3 hours to obtain the optical lens capable of shielding harmful light and correcting vision.

[0116] Experimental example

[0117] Optical lenses capable of shielding harmful light and correcting vision prepared in Example 5 and Comparative Examples 1 to 2 are obtained respectively;

[0118] The light transmittance of the above-mentioned different optical lenses was tested using an ultraviolet-visible light photometer, and the test results are shown in Table 1:

[0119] Table 1

[0120]

[0121] From Table 1, we can see that:

[0122] Compared with the comparative example, the optical lens capable of shielding harmful light and correcting vision prepared in the embodiment of the present application has excellent light transmittance and blue light and ultraviolet protection performance.

[0123] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. An optical lens capable of shielding harmful light and correcting vision, characterized in that: The optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage: Epoxy resin 3% to 5%, nano iron oxide 0.5% to 1.2%, carbon nanotube 0.5% to 1%, ultraviolet absorber 1% to 4%, initiator 1% to 1.5%, and the balance is CR39 resin monomer.

2. The optical lens capable of shielding harmful light and correcting vision according to claim 1, characterized in that: The optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage: Epoxy resin 3.5%-4.5%, nano iron oxide 0.8%-1.0%, carbon nanotube 0.6%-0.8%, ultraviolet absorber 2%-3%, initiator 1.2%-1.5%, and the balance is CR39 resin monomer.

3. The optical lens capable of shielding harmful light and correcting vision according to claim 1, characterized in that: The optical lens capable of shielding harmful light and correcting vision comprises the following raw materials in percentage: Epoxy resin 4%, nano iron oxide 1%, carbon nanotubes 0.8%, ultraviolet absorber 3%, initiator 1.2%, and the balance is CR39 resin monomer.

4. The optical lens capable of shielding harmful light and correcting vision according to claim 1, characterized in that: The ultraviolet absorber is selected from at least one of UV-P, UV-327, UV-360 and UV-928.

5. The optical lens capable of shielding harmful light and correcting vision according to claim 1, characterized in that: The initiator is diisopropyl peroxydicarbonate.

6. The method for preparing an optical lens capable of shielding harmful light and correcting vision as claimed in any one of claims 1 to 5, characterized in that: The steps include: (a) weighing each raw material according to weight; (b) mixing CR39 resin monomer, epoxy resin, nano iron oxide, carbon nanotubes and ultraviolet absorber to obtain a mixture; (c) adding an initiator to the mixture for heating reaction to obtain a reactant; (d) adding the reactants into a mold for heating and curing, demolding, and continuing heating for secondary curing to obtain the optical lens capable of shielding harmful light and correcting vision.

7. The preparation method according to claim 6, characterized in that: In the step (c), the heating reaction temperature is 50-60° C. and the reaction time is 2-3 hours.

8. The preparation method according to claim 6, characterized in that: In the step (d), the heating curing is to raise the temperature to 85° C. within 16 to 18 hours.

9. The preparation method according to claim 6, characterized in that: In the step (d), the secondary curing temperature is 125-130° C. and the time is 2-3 hours.