Al (OH) 3 modified calcium sulfate whisker / epoxy resin heat-conducting composite material and preparation method thereof
Through the preparation method of Al(OH)3 modified calcium sulfate whiskers and epoxy resin composite material, the problems of poor thermal conductivity and high preparation cost of epoxy resin are solved, and high thermal conductivity and low cost thermal conductivity are achieved. In the thermal management of electronic components.
Patent Information
- Application Number
- CN202411385857.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The existing epoxy resins have poor thermal conductivity and high production cost, making it difficult to meet the application requirements of high thermal conductivity requirements. Commonly used thermal fillers such as aluminum hydroxide and alumina are granular, which limits the development and cost control of thermally conductive composite materials.
Using the composite material preparation method of Al(OH)3 modified calcium sulfate whiskers and epoxy resin, Al(OH)3 modified calcium sulfate whiskers are used to react with calcium sulfate whiskers with octadecyl sulfate and urea to form Al(OH)3 modified calcium sulfate whiskers. It is mixed with components such as epoxy resin, curing agent, etc., and the thermally conductive composite material is prepared by ultrasonic dispersion and heating curing.
It significantly improves the thermal conductivity of thermal composite materials, up to 1.16 W m-1K-1, 480% higher than pure epoxy resin, and reduces the preparation cost. The material has good electrical insulation and plasticity. Suitable for thermal management of electronic components.
Smart Images

Figure CN119060503A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal conductive composite material synthesis methods, and specifically relates to an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material and a preparation method thereof. Background Art
[0002] Electronic devices usually generate continuous heat accumulation during operation, which needs to be removed through conduction or heat dissipation. Using thermal conductive materials is one of the effective ways to solve this problem. Generally speaking, polymer materials have poor thermal conductivity, generally 0.2 W m -1 K -1 A composite method is often used to improve its thermal conductivity. For example, the introduction of fillers such as aluminum hydroxide, aluminum oxide, and boron nitride can build a thermal conductive path inside the resin matrix to improve the thermal conductivity of the polymer material.
[0003] Generally speaking, thermal conductive fillers with large aspect ratios are more likely to form interconnected thermal conductive paths inside the resin matrix. Commonly used thermal conductive fillers such as aluminum hydroxide, aluminum oxide, and boron nitride are all in granular form, which limits the development of thermal conductive composite materials. In addition, the unit price of matrix fillers is generally high, which increases the cost of composite materials and makes it difficult to promote their application.
[0004] In view of the technical problems of poor thermal conductivity and high preparation cost of existing epoxy resins, it is urgently necessary to conduct modification research on them to improve the thermal conductivity of epoxy resin composites so that they can meet the application requirements of high thermal conductivity requirements, reduce the overall cost of composite materials, and improve their market competitiveness. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material and a preparation method thereof, so as to solve the technical problems of poor thermal conductivity of epoxy resin and high preparation cost.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions: The invention discloses a method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, comprising the following steps: 1) Ultrasonic dispersion of calcium sulfate whiskers in deionized water, followed by addition of aluminum sulfate 18hydrate and stirring until completely dissolved, addition of urea and heating and stirring, followed by suction filtration, washing and drying to obtain Al(OH)3 modified calcium sulfate whiskers; 2) The Al(OH)3 modified calcium sulfate whisker prepared in step 1) is added to butyl acetate / n-butanol solvent, and after ultrasonic dispersion, epoxy resin, curing agent, leveling agent, dispersant, defoaming agent and anti-settling agent are added. After stirring, the mixture is poured into a mold and heated to be cured to obtain an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material.
[0007] Preferably, in step 1), the mass ratio of calcium sulfate whiskers: urea: aluminum sulfate 18hydrate: deionized water is 1: (0.9-2.7): (1.6-4.8): (25-75).
[0008] Preferably, in step 1), the heating and stirring temperature is 80-95°C for 3-5 h; the drying conditions are: drying at 80-95°C for 8 h, and then drying at 200-220°C for 2 h.
[0009] Preferably, in step 1), the calcium sulfate whiskers are prepared from gypsum or industrial by-product gypsum, and have an aspect ratio of 20-30.
[0010] Preferably, in step 2), the mass ratio of Al(OH)3 modified calcium sulfate whiskers: butyl acetate / n-butanol solvent is 1:(1-3): epoxy resin: curing agent: defoaming agent: dispersant: anti-settling agent: leveling agent is 1:(1-3):(0.5-1.3):(0.1-1):(0.005-0.015):(0.01-0.015):(0.005-0.015):(0.005-0.015).
[0011] Preferably, in step 2), the butyl acetate / n-butanol solvent is prepared by mixing butyl acetate and n-butanol; the mass ratio of butyl acetate to n-butanol is 1:1.
[0012] Preferably, in step 2), the epoxy resin is at least one of E-51, E-44 and E-20; the curing agent is polyamide; the leveling agent is BYK-333; the dispersant is BYK-110; the defoaming agent is BYK-141; and the anti-settling agent is BYK-410.
[0013] Preferably, in step 2), the mass ratio of Al(OH)3 modified calcium sulfate whisker to Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material is (0.3-0.6):1.
[0014] Preferably, in step 2), the conditions for heating and curing are: heating at 45°C for 6 h, heating at 60°C for 4 h, heating at 80°C for 3 h, heating at 100°C for 2 h, and heating at 120°C for 1 h.
[0015] The present invention also discloses an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, which is prepared by the above preparation method and has a maximum thermal conductivity of 1.16 W m -1 K -1 The thermal conductivity of pure epoxy resin is increased by 480%; the volume resistivity is 10 12 Ω m or more; surface resistivity is 10 12 Ω m or more.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention discloses a method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material. First, by using calcium sulfate whiskers as raw materials, the product performance and structure are more stable. By introducing calcium sulfate whiskers into the epoxy resin matrix, the internal structure of the matrix is optimized, and the microstructure of the obtained thermal conductive composite material is more compact. Second, by loading Al(OH)3 on the surface of inorganic particles, CSW can have good thermal conductivity and insulation, which can improve thermal management in thermal interface materials for electronic packaging. Third, calcium sulfate whiskers are mainly distributed in the matrix material in a flaky form, which can increase the thermal conductive interface and thermal contact points in the matrix, construct a thermal conductive path, and reduce the thermal resistance of the material interface. Fourth, the introduction of calcium sulfate whiskers can significantly reduce the preparation cost of thermal conductive insulating materials and meet actual production needs.
[0017] The present invention also discloses an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material prepared by the above preparation method, which can obtain a maximum thermal conductivity of 1.16 W m -1 K -1 The high thermal conductivity of PE is 0.20 W m -1 K -1 ), its thermal conductivity increased by 480%. At the same time, the composite material has 10 12 The volume / surface resistivity of Ω m or above has good electrical insulation. This is because the material has a dense internal structure, obvious thermal conductivity, good insulation, plasticity, and light weight. The contact thermal conductive filler forms a thermal conductive path, which can effectively dissipate heat and conduct heat to maintain the normal operating temperature and performance of electronic components. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The microscopic morphology and energy spectrum diagram of the Al(OH)3 modified calcium sulfate whisker (Al(OH)3@CSW) disclosed in Example 1 of the present invention; wherein, (a) is the energy spectrum analysis diagram of Al(OH)3@CSW; (b) is the SEM diagram of Al(OH)3@CSW; (c) the distribution diagram of the Ca element; (d) the distribution diagram of the S element; (e) the distribution diagram of the O element; (f) the distribution diagram of the Al element; Figure 2 The relationship between the thermal conductivity and filler content of the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material disclosed in the present invention; Figure 3 The present invention discloses a graph showing the relationship between the surface resistivity, volume resistivity, breakdown voltage and electrical strength of the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material and the filler content; wherein (a) is a graph showing the relationship between the surface resistivity and volume resistivity and the filler content; and (b) is a graph showing the relationship between the breakdown voltage and electrical strength and the filler content. DETAILED DESCRIPTION
[0019] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0020] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0021] The present invention is further described in detail below in conjunction with the accompanying drawings: Calcium sulfate whiskers (CSW) have attracted much attention due to their unique morphology, good compatibility and economical price. Relevant reports suggest that the introduction of calcium sulfate whiskers can significantly improve the mechanical properties of composite materials, and the commercial unit price of this material is almost the lowest among all inorganic fillers. Secondly, because calcium sulfate whiskers have a large aspect ratio and different morphologies, when the whiskers are dispersed in the composite matrix, they are easy to contact each other to form an interconnected contact network structure, thereby promoting the improvement of thermal conductivity. Aluminum oxide is a material with good thermal conductivity and a high thermal conductivity coefficient. When aluminum oxide is loaded on the surface of inorganic particles, the thermal conductivity of aluminum can be fully utilized to quickly transfer heat. This is because inorganic particles usually have a large surface area, and aluminum oxide loading can provide more heat transfer interfaces and enhance the thermal conductivity effect. Secondly, inorganic particles generally have a high heat capacity. When receiving heat, their temperature rises, they can store more heat, and can better absorb, transfer and release heat under different environments. Therefore, it is considered to load aluminum oxide on the surface of flaky calcium sulfate whiskers to improve thermal conductivity by increasing the number of thermal contact points and interfaces. However, previous research on loading aluminum oxide on flaky whiskers is almost invisible, and a suitable route needs to be explored, which is challenging.
[0022] The invention discloses a method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, comprising the following steps: 1) Add calcium sulfate whiskers to a beaker filled with deionized water and disperse them by ultrasonic dispersion, then add aluminum sulfate 18hydrate, stir until completely dissolved, add urea, heat and stir at 80-95°C for 3-5 h, filter and wash, dry at 80-95°C for 8 h, and then dry at 200-220°C for 2 h to obtain Al(OH)3 modified calcium sulfate whiskers; 2) Mixing butyl acetate and n-butanol solvent to prepare butyl acetate / n-butanol solvent; placing the Al(OH)3 modified calcium sulfate whisker prepared in step 1) in a glass bottle containing butyl acetate / n-butanol solvent to obtain a mixed solution; dispersing the mixed solution by ultrasonic treatment for 30 min, adding epoxy resin, curing agent, leveling agent, dispersant, defoaming agent and anti-settling agent into the bottle in proportion, stirring in an agitator for 5 h, pouring into a mold, heating and curing, and obtaining an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material.
[0023] In a preferred embodiment of the present invention, in step 1), the calcium sulfate whiskers are prepared from gypsum or industrial by-product gypsum, and have an aspect ratio of 20 to 30.
[0024] The mass ratio of calcium sulfate whiskers: urea: aluminum sulfate 18hydrate: deionized water is 1: (0.9~2.7): (1.6~4.8): (25~75).
[0025] In step 2), the mass ratio of Al(OH)3 modified calcium sulfate whisker: butyl acetate / n-butanol solvent: epoxy resin: curing agent: defoaming agent: dispersant: anti-settling agent: leveling agent is 1:(1-3):(0.5-1.3):(0.1-1):(0.005-0.015):(0.01-0.015):(0.005-0.015):(0.005-0.015); the butyl acetate / n-butanol solvent is prepared by mixing butyl acetate and n-butanol, wherein the mass ratio of butyl acetate:n-butanol is 1:1.
[0026] The mass ratio of Al(OH)3 modified calcium sulfate whiskers to butyl acetate / n-butanol solvent is 1:(1~3).
[0027] In step 3), the epoxy resin is at least one of E-51, E-44 and E-20; the curing agent is polyamide; the leveling agent is BYK-333; the dispersant is BYK-110; the defoaming agent is BYK-141; and the anti-settling agent is BYK-410.
[0028] The mass ratio of Al(OH)3 modified calcium sulfate whisker to Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material is (0.3~0.6):1.
[0029] In step 2), the heating and curing conditions are as follows: heat at 45°C on a heating table for 6 h, then heat in an oven in a stepwise manner, heating at 60°C for 4 h, 80°C for 3 h, 100°C for 2 h, and 120°C for 1 h to obtain an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material.
[0030] The present invention also discloses a thermally conductive composite material obtained by the above preparation method, which can obtain a maximum thermal conductivity of 1.16 W m -1 K -1 The high thermal conductivity of PE is 0.20 W m -1 K -1 ), its thermal conductivity increased by 480%. At the same time, the composite material has 10 12 The volume resistivity and surface resistivity above Ωm have good electrical insulation. This is because the material has a dense internal structure, obvious thermal conductivity, good insulation, plasticity, and light weight. The contact thermal conductive filler forms a thermal conductive path, which can effectively dissipate heat and conduct heat to maintain the normal operating temperature and performance of electronic components.
[0031] Example 1 A method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that it comprises the following steps: Step 1. Weigh 1 part of calcium sulfate whisker with an aspect ratio of 20, add it to 25 parts of deionized water, and ultrasonicate for 30 minutes to obtain a suspension; then add 1.6 parts of aluminum sulfate 18hydrate and stir until dissolved; then add 0.9 parts of urea, continue heating and stirring at 80°C for 5 hours after the addition is complete, then filter while hot, wash with deionized water and centrifuge 5 times, place the centrifuged product in an oven at 80°C and dry for 8 hours, then heat to 200°C and dry for 2 hours to obtain modified calcium sulfate whiskers for later use.
[0032] Step 2: Prepare a mixed solvent of butyl acetate and n-butanol in a ratio of 1:1. Weigh 1 part of Al(OH)3@CSW composite whiskers and 3 parts of the mixed solvent into a glass bottle.
[0033] Step 3: After ultrasonically dispersing the solution in the glass bottle, add 1.3 parts of epoxy resin E-44 and 1.0 parts of polyamide curing agent, and then add 0.01 parts of dispersant BYK-110, 0.005 parts of leveling agent BYK-333, 0.005 parts of defoaming agent BYK-141 and anti-settling agent BYK-410. After stirring for 5 hours, use a rotary evaporator to remove the solvent without causing a cross-linking reaction, place it on a heating table and heat it at 45°C for 6 hours, and then stepwise heat the oven (heating at 60°C for 4 hours, 80°C for 3 hours, 100°C for 2 hours, and 120°C for 1 hour) to obtain a composite material.
[0034] The thermally conductive composite material prepared by the above preparation method has an interconnected network of composite whiskers in the matrix that can effectively conduct heat. The thermal conductivity of the Al(OH)3@CSW-30 / EP composite material reaches 0.41 W m -1 K -1 , compared with pure EP (0.20 W m -1 K -1 ), its thermal conductivity increased by 105%. At the same time, the volume or surface resistivity of the composite material is higher than 10 12 Ω cm, the tensile strength reaches 37.3MPa, which is 38% higher than that of pure EP (27 MPa), and the breakdown strength is 16.6 KV / mm, which is 98% higher than that of pure EP (8.4KV / mm).
[0035] See also Figure 1The microscopic morphology and energy spectrum of the Al(OH)3 modified calcium sulfate whisker (Al(OH)3@CSW) disclosed in Example 1 of the present invention; wherein, (a) is the energy spectrum analysis diagram of Al(OH)3@CSW; (b) is the SEM diagram of Al(OH)3@CSW; (c) the distribution diagram of the Ca element; (d) the distribution diagram of the S element; (e) the distribution diagram of the O element; (f) the distribution diagram of the Al element; it can be clearly observed from the figure that a dense layer of fine particles is wrapped on the originally smooth surface of CSW. Combining the energy spectrum analysis and mapping element distribution results, it can be seen that the distribution of Al and O elements is completely consistent with the distribution profile of the Ca element, and it can be concluded that this fine particle is Al(OH)3. Through morphological structure analysis, it can be seen that Al(OH)3 can be successfully loaded on the surface of CSW, that is, Al(OH)3@CSW composite whiskers are successfully prepared. The prepared insulating thermal conductive composite material can obtain a maximum of 1.16 W m -1 K -1 The high thermal conductivity of pure EP (0.20 W m -1 K -1 ), its thermal conductivity increased by 480%. At the same time, the composite material has 10 12 The volume or surface resistivity is above Ω cm, and it has good electrical insulation. It can effectively conduct heat to maintain the normal operating temperature and performance of electronic components.
[0036] Example 2 A method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that it comprises the following steps: Step 1. Weigh 1 part of calcium sulfate whisker with an aspect ratio of 25, add it to 75 parts of deionized water, and ultrasonicate for 30 minutes to obtain a suspension; then add 4.8 parts of aluminum sulfate 18hydrate and stir until dissolved; then add 2.7 parts of urea, continue heating and stirring at 95°C for 3 hours after the addition is complete, then filter while hot, wash with deionized water and centrifuge 5 times, place the centrifuged product in a 90°C oven and dry it for 8 hours, then heat to 210°C and dry it for 2 hours to obtain modified calcium sulfate whiskers for later use.
[0037] Step 2: Prepare a mixed solvent of butyl acetate and n-butanol in a ratio of 1:1. Weigh 1 part of Al(OH)3@CSW composite whiskers and 2 parts of the mixed solvent into a glass bottle.
[0038] Step 3: After ultrasonically dispersing the solution in the glass bottle, add 0.8 parts of epoxy resin E-44 and 0.7 parts of polyamide curing agent, and then add 0.01 parts of dispersant BYK-110, 0.005 parts of leveling agent BYK-333, 0.005 parts of defoaming agent BYK-141 and BYK-410 anti-settling agent. After stirring for 5 hours, use a rotary evaporator to remove the solvent without causing a cross-linking reaction, place it on a heating table and heat it at 45°C for 6 hours, and then stepwise heat the oven (heating at 60°C for 4 hours, 80°C for 3 hours, 100°C for 2 hours, and 120°C for 1 hour) to obtain a composite material.
[0039] A thermally conductive composite material prepared by the above preparation method has remarkable application performance and characteristics. The thermal conductivity of the Al(OH)3@CSW-40 / EP composite material reaches 0.52 W m -1 K -1 , compared with pure EP (0.20 W m -1 K -1 ), its thermal conductivity increased by 160%. At the same time, the volume or surface resistivity of the composite material is higher than 10 12 Ω cm, the tensile strength reaches 40.2MPa, which is 49% higher than that of pure EP (27 MPa), and the breakdown strength is 16.2 KV / mm, which is 97% higher than that of pure EP (8.4KV / mm).
[0040] Example 3 A method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that it comprises the following steps: Step 1. Weigh 1 part of calcium sulfate whisker with an aspect ratio of 30, add it to 50 parts of deionized water, and ultrasonicate for 30 minutes to obtain a suspension; then add 3.2 parts of aluminum sulfate 18hydrate and stir until dissolved; then add 1.8 parts of urea, continue heating and stirring at 90°C for 4 hours after the addition is complete, then filter while hot, wash with deionized water and centrifuge 5 times, place the centrifuged product in an oven at 85°C and dry for 8 hours, then heat to 215°C and dry for 2 hours to obtain modified calcium sulfate whiskers for later use.
[0041] Step 2: Prepare a mixed solvent of butyl acetate and n-butanol in a ratio of 1:1. Weigh 1 part of Al(OH)3@CSW composite whisker and 1 part of the mixed solvent and place them in a glass bottle.
[0042] Step 3: After ultrasonically dispersing the solution in the glass bottle, add 0.5 parts of epoxy resin E-51 and 0.5 parts of polyamide curing agent, and then add 0.012 parts of dispersant BYK-110, 0.01 parts of leveling agent BYK-333 and 0.01 parts of defoaming agent BYK-141 and BYK-410 anti-settling agent. After stirring for 1 hour, use a rotary evaporator to remove the solvent without producing a cross-linking reaction, place it on a heating table and heat it at 45°C for 6 hours, and then stepwise heat the oven (heating at 60°C for 4 hours, 80°C for 3 hours, 100°C for 2 hours, and 120°C for 1 hour) to obtain a composite material.
[0043] The thermally conductive composite material prepared by the above preparation method has remarkable application performance and characteristics. The interconnected network formed by the composite whiskers in the matrix can effectively conduct heat. The thermal conductivity of the Al(OH)3@CSW-50 / EP composite material reaches 0.63 W m -1 K -1 , compared with pure EP (0.20 W m -1 K -1 ), its thermal conductivity increased by 215%. At the same time, the volume or surface resistivity of the composite material is higher than 10 12 Ω cm, the tensile strength reaches 38.1MPa, which is 41% higher than that of pure EP (27 MPa), and the breakdown strength is 11.2 KV / mm, which is 32% higher than that of pure EP (8.4KV / mm).
[0044] Example 4 A method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that it comprises the following steps: Step 1, weigh 1 part of calcium sulfate whisker with an aspect ratio of 30, add it to 25 parts of deionized water, and ultrasonicate for 30 minutes to obtain a suspension; then add 3.2 parts of aluminum sulfate 18hydrate and stir until dissolved; then add 2.7 parts of urea, continue heating and stirring at 85°C for 4.5 hours after the addition is complete, then filter while hot, wash with deionized water and centrifuge 5 times, place the centrifuged product in a 95°C oven and dry it for 8 hours, then heat to 200°C and dry it for 2 hours to obtain modified calcium sulfate whiskers for later use.
[0045] Step 2: Prepare a mixed solvent of butyl acetate and n-butanol in a ratio of 1:1. Weigh 1 part of Al(OH)3@CSW composite whisker and 1 part of the mixed solvent and place them in a glass bottle.
[0046] Step 3: After ultrasonically dispersing the solution in the glass bottle, add 0.56 parts of epoxy resin E-20 and 0.1 parts of polyamide curing agent, and then add 0.015 parts of dispersant BYK-110 and leveling agent BYK-333, 0.015 parts of defoaming agent BYK-141 and BYK-410 anti-settling agent. After stirring for 5 hours, use a rotary evaporator to remove the solvent without producing a cross-linking reaction, place it on a heating table and heat it at 45°C for 6 hours, and then stepwise heat the oven (heating at 60°C / 4 hours, 80°C for 3 hours, 100°C for 2 hours, and 120°C for 1 hour) to obtain a composite material.
[0047] The thermally conductive composite material prepared by the above preparation method has remarkable application performance and characteristics. The interconnected network formed by the composite whiskers in the matrix can effectively conduct heat. The thermal conductivity of the Al(OH)3@CSW-60 / EP composite material reaches 1.16 W m -1 K -1 , compared with pure EP (0.20 W m -1 K -1 ), its thermal conductivity increased by 480%. At the same time, the volume or surface resistivity of the composite material is higher than 10 12 Ω cm, the tensile strength reaches 32.1MPa, which is 19% higher than that of pure EP (27 MPa), and the breakdown strength is 8.6 KV / mm, which is 2% higher than that of pure EP (8.4KV / mm).
[0048] Example 5 A method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that it comprises the following steps: A method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that it comprises the following steps: Step 1. Weigh 1 part of calcium sulfate whisker with an aspect ratio of 25, add it to 60 parts of deionized water, and ultrasonicate for 30 minutes to obtain a suspension; add 4.0 parts of aluminum sulfate 18hydrate thereto, stir until dissolved, and then add 2.4 parts of urea. After the addition is completed, continue to heat and stir at 92°C for 3.5 hours, then filter while hot, wash with deionized water and centrifuge 5 times, place the centrifuged product in a 90°C oven to dry for 8 hours, then heat to 220°C and dry for 2 hours to obtain modified calcium sulfate whiskers for later use.
[0049] Step 2: Prepare a mixed solvent of butyl acetate and n-butanol in a ratio of 1:1. Weigh 1 part of Al(OH)3@CSW composite whiskers and 2 parts of the mixed solvent into a glass bottle.
[0050] Step 3: After ultrasonically dispersing the solution in the glass bottle, add 0.8 parts of epoxy resin E-44 and 0.7 parts of polyamide curing agent, and then add 0.012 parts of dispersant BYK-110, 0.008 parts of leveling agent BYK-333, 0.008 parts of defoaming agent BYK-141 and BYK-410 anti-settling agent. After stirring for 5 hours, use a rotary evaporator to remove the solvent without causing a cross-linking reaction, place it on a heating table and heat it at 45°C for 6 hours, and then stepwise heat the oven (heating at 60°C for 4 hours, 80°C for 3 hours, 100°C for 2 hours, and 120°C for 1 hour) to obtain a composite material.
[0051] A thermally conductive composite material prepared by the above preparation method has remarkable application performance and characteristics. The thermal conductivity of the Al(OH)3@CSW-40 / EP composite material reaches 0.51 W m -1 K -1 .
[0052] Comparison example A method for preparing an epoxy resin thermally conductive composite material, characterized in that it comprises the following steps: Step 1: prepare a mixed solvent of butyl acetate and n-butanol in a ratio of 1:1.
[0053] Step 2: Add 5 parts of epoxy resin E-44, 4 parts of polyamide curing agent and 3 parts of mixed solvent into a glass bottle, remove the solvent using a rotary evaporator without producing a cross-linking reaction, and then heat it on a heating table at 45°C for 6 h, and then heat it in an oven in a stepwise manner (heating at 60°C for 4 h, 80°C for 3 h, 100°C for 2 h, and 120°C for 1 h to obtain a composite material.
[0054] The epoxy resin material prepared by the above preparation method has the remarkable application performance and characteristic of excellent electrical insulation. The prepared insulating material obtains 0.20 W m -1 K -1 The thermal conductivity is 10 14 The volume or surface resistivity is above Ω cm, which has good electrical insulation. At the same time, the material has a tensile strength of 27 MPa and a breakdown strength of 8.4 KV / mm.
[0055] Figure 2 The relationship between the thermal conductivity and filler content of the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material of Example 1 disclosed in the present invention; it can be seen from the figure that with the increase of the addition amount of the modified whisker, the thermal conductivity of the composite material is gradually improved. When the addition amount of the Al(OH)3 modified calcium sulfate whisker is 60%, the thermal conductivity of the composite material can reach 1.16 W m -1 K-1 .
[0056] Figure 3 The relationship between the surface resistivity, volume resistivity, breakdown voltage and electrical strength and the filler content of the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material of Example 1 disclosed in the present invention; wherein, (a) is a relationship diagram between the breakdown voltage and electrical strength and the filler content; (b) is a relationship diagram between the surface resistivity and volume resistivity and the filler content; it can be seen from the figure that the addition of modified whiskers can effectively improve the pressure resistance of the composite material, and the surface resistivity and volume resistivity of the composite material after the whiskers are added are not greatly reduced, and are still maintained at 10 14 cm, showing good insulation properties.
[0057] The present invention discloses an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material and a preparation method thereof. Calcium sulfate whiskers are added to an aqueous solution of urea and aluminum sulfate 18hydrate, and Al(OH)3 modified calcium sulfate whiskers are obtained by heating and stirring. The calcium sulfate whiskers are then dispersed in a mixed solution of epoxy resin and a curing agent, and the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material is prepared by casting and molding. The prepared thermal conductive composite material has a dense internal structure, an obvious thermal conductive effect, good insulation, plasticity, and light weight, and can effectively dissipate heat and conduct heat to maintain the normal operating temperature and performance of electronic components. The Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material has good heat dissipation and insulation effects when used in electronic component integrated circuits. When used in electronic products, it can effectively guide heat outflow and reduce the risk of overheating during the operation of electronic components.
[0058] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that: The following steps are involved: 1) Ultrasonic dispersion of calcium sulfate whiskers in deionized water, followed by addition of aluminum sulfate 18hydrate and stirring until completely dissolved, addition of urea and heating and stirring, followed by suction filtration, washing and drying to obtain Al(OH)3 modified calcium sulfate whiskers; 2) The Al(OH)3 modified calcium sulfate whisker prepared in step 1) is added to butyl acetate / n-butanol solvent, and after ultrasonic dispersion, epoxy resin, curing agent, leveling agent, dispersant, defoaming agent and anti-settling agent are added. After stirring, the mixture is poured into a mold and heated to be cured to obtain an Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material.
2. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 1), the mass ratio of the calcium sulfate whisker: urea: aluminum sulfate 18hydrate: deionized water is 1: (0.9-2.7): (1.6-4.8): (25-75).
3. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 1), the heating and stirring temperature is 80-95°C for 3-5 hours; the drying conditions are: drying at 80-95°C for 8 hours, and then drying at 200-220°C for 2 hours.
4. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 1), the calcium sulfate whiskers are prepared from gypsum or industrial by-product gypsum, and have an aspect ratio of 20-30.
5. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 2), the mass ratio of the Al(OH)3 modified calcium sulfate whisker: butyl acetate / n-butanol solvent is 1:(1-3): epoxy resin: curing agent: defoaming agent: dispersant: anti-settling agent: leveling agent is 1:(1-3):(0.5-1.3):(0.1-1):(0.005-0.015):(0.01-0.015):(0.005-0.015):(0.005-0.015).
6. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 2), the butyl acetate / n-butanol solvent is prepared by mixing butyl acetate and n-butanol; the mass ratio of butyl acetate to n-butanol is 1:
1.
7. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 2), the epoxy resin is at least one of E-51, E-44 and E-20; the curing agent is polyamide; the leveling agent is BYK-333; the dispersant is BYK-110; the defoaming agent is BYK-141; and the anti-settling agent is BYK-410.
8. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 2), the mass ratio of Al(OH)3 modified calcium sulfate whisker to Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material is (0.3~0.6):
1.
9. The method for preparing the Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material according to claim 1, characterized in that: In step 2), the heating and curing conditions are: heating at 45°C for 6 h, heating at 60°C for 4 h, heating at 80°C for 3 h, heating at 100°C for 2 h, and heating at 120°C for 1 h.
10. An Al(OH)3 modified calcium sulfate whisker / epoxy resin thermal conductive composite material, characterized in that: The preparation method according to any one of claims 1 to 9 is used, and the maximum thermal conductivity is 1.16 W m -1 K -1 The thermal conductivity of pure epoxy resin is increased by 480%; the volume resistivity is 10 12 Ω m or more; surface resistivity is 10 12 Ω m or more.
Citation Information
Patent Citations
Calcium sulfate whisker / epoxy resin composite filter material and preparation method thereof
CN104559065A
Method for modifying calcium sulphate whisker surface
CN104651945A
Binary composite fiber reinforced epoxy resin-based rapid repair material and preparation method thereof
CN117923832A
Heat-conducting high-temperature-resistant sealing coating material and preparation method thereof
CN118546592A