Low-cost conductive silicone rubber and preparation process thereof

By preparing modified conductive filler powder, the modified silane coupling agent is generated by reacting cystine perfluorinated derivatives with KH-560, grafting to the surface of acetylene carbon black, combined with graphite, and self-healing properties of conductive silicone rubber are solved. The poor problem has achieved low-cost and high-performance conductive silicone rubber preparation, improving the conductive and mechanical properties.

CN119060544APending Publication Date: 2024-12-03CHUZHOU JUNYUE MACROMOLECULE NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411374223.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The self-repairing performance of existing conductive silicone rubber is poor, and when using metal powder or acetylene carbon black as conductive additives, the cost is high, the processing is difficult, and the mechanical performance of the product is poor.

Method used

Modified conductive filler powder is used to react cystine perfluorinated derivatives with KH-560 to form a modified silane coupling agent, grafted to the surface of acetylene carbon black, combined with graphite, and form a disulfide bond, ester group and fluorine. The modified conductive filler powder of the alkyl chain improves the self-healing ability and conductive properties of conductive silicone rubber.

Benefits of technology

It reduces material costs, improves the conductive properties, mechanical properties and self-repairing properties of conductive silicone rubber, and ensures the self-repairing ability of conductive silicone rubber under heating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068302880000091
    Figure BDA0005068302880000091
Patent Text Reader

Abstract

The invention discloses low-cost conductive silicone rubber and a preparation process thereof, and belongs to the technical field of silicone rubber, and the obtained low-cost conductive silicone rubber comprises the following raw materials in parts by weight: 94-98 parts of methyl vinyl silicone rubber, 30-50 parts of modified conductive filling powder, 1-2 parts of a vulcanization accelerator and 1-2 parts of a release agent. The preparation process of the low-cost conductive silicone rubber comprises the following steps: putting the methyl vinyl silicone raw rubber and the conductive filling powder into an internal mixer, mixing for 15-30 minutes, then putting the vulcanization accelerator and the release agent into the internal mixer, mixing for 30-50 minutes, and pouring out the materials in the internal mixer to obtain the low-cost conductive silicone rubber. The conductive silicone rubber prepared by the preparation method disclosed by the invention has excellent conductivity and self-repairing performance while the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicone rubber, and in particular relates to low-cost conductive silicone rubber and a preparation process thereof. Background Art

[0002] Silicone rubber is a polymer composed of (—Si—O—)n as its main chain and organic groups as its side groups. It exhibits excellent heat resistance, low-temperature resistance, weather resistance, UV resistance, and biological properties. Due to the high flexibility of silicone rubber's molecular chains and the weak interactions between them, vulcanized silicone rubber is soft and elastic. Furthermore, because it does not contain softeners, plasticizers, or antioxidants, it does not cause environmental pollution, making it ideal for use as a material in electronic components.

[0003] Current conductive silicone rubbers are typically prepared by adding conductive additives (such as metal powder and acetylene black), structure control agents, and vulcanizing agents to a silicone rubber base to meet electrical and mechanical performance requirements. However, this preparation method has significant drawbacks. Using metal powder as a conductive additive is costly, difficult to process, and results in poor mechanical properties. Using acetylene black as a conductive additive results in slow vulcanization, mold sticking, and significant product deformation. Patent CN112210215B discloses a conductive silicone rubber with low tensile permanent deformation and a preparation method thereof. The conductive silicone rubber prepared by this patent comprises methyl vinyl silicone rubber raw rubber, methyl silicone rubber raw rubber, white carbon black, acetylene carbon black, silane coupling agent, hydroxy silicone oil, methyl silicone oil, hydrogen-containing silicone oil, vulcanizing agent, and zinc stearate. The preparation steps include: placing the raw materials into a kneader to prepare a mixed base rubber; adding acetylene carbon black, methyl silicone oil, and methyl silicone rubber raw rubber after the mixed base rubber is cooled, heating and stirring to produce a rubber material; after the rubber material is allowed to stand and cool, adding a vulcanizing agent on a double roller; and molding the conductive silicone rubber containing the vulcanizing agent and performing a secondary vulcanization to obtain a product. However, the conductive silicone rubber prepared by this patent and the prior art still has the disadvantage of poor self-healing performance. Summary of the Invention

[0004] In order to solve the disadvantage that the conductive silicone rubber prepared by the prior art still has poor self-healing performance, the purpose of the present invention is to provide a low-cost conductive silicone rubber and a preparation process thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A low-cost conductive silicone rubber comprises the following raw materials in parts by weight: 94-98 parts of methyl vinyl silicone rubber, 30-50 parts of modified conductive filling powder, 1-2 parts of a vulcanization accelerator, and 1-2 parts of a release agent.

[0007] Furthermore, the molecular weight of the methyl vinyl silicone rubber is 600,000-700,000, and the vinyl molar content is 0.03%-0.05%.

[0008] Furthermore, the preparation method of the modified conductive filler powder is:

[0009] Step A1: Add cystine, 1H,1H-perfluoro-1-octanol, p-toluenesulfonic acid, and toluene to a reaction flask and stir; heat to 112°C, reflux for 3 hours, cool to -5 to 5°C in a water bath, and keep warm for 1 hour; filter, wash with frozen toluene, and dry to obtain a perfluorinated cystine derivative;

[0010] The usage ratio of cystine, 1H,1H-perfluoro-1-octanol, p-toluenesulfonic acid and toluene is 24g:80g:2-4g:1-1.2L.

[0011] In the above steps, p-toluenesulfonic acid is used as a catalyst to catalyze the esterification reaction between the carboxyl group of cystine and the hydroxyl group of 1H,1H-perfluoro-1-octanol to obtain a perfluorinated cystine derivative containing an ester group, a disulfide bond, a fluoroalkyl chain, and an amino group.

[0012] Step A2: uniformly mix the perfluorinated derivative of cystine and KH-560, and react at 40° C. for 30 min to obtain a modified silane coupling agent;

[0013] The mass ratio of the perfluorinated cystine derivative to KH-560 is 20:4.7.

[0014] In the above steps, the amino group of the perfluorinated cystine derivative undergoes a ring-opening reaction with the epoxy group of KH-560 to obtain a modified silane coupling agent.

[0015] Step A3: adding acetylene black, graphite, and a modified silane coupling agent to an ethanol aqueous solution, stirring at 8000 rpm for 20-30 minutes, and drying at 80° C. for 12 hours to obtain a modified conductive filler powder;

[0016] The dosage ratio of acetylene carbon black, graphite, modified silane coupling agent and ethanol aqueous solution is 3-6 g: 3-6 g: 0.03-0.06 g: 150 mL; the volume ratio of anhydrous ethanol and deionized water in the ethanol aqueous solution is 9:1.

[0017] Through the above steps, a modified silane coupling agent containing disulfide bonds, ester groups, hydroxyl groups, and fluoroalkyl chains is grafted onto the surface of acetylene carbon black. Compared with conventional covalent bonds such as CC, COC, and CN, the bond energy of disulfide bonds is lower and can be broken or undergo reversible reactions under external stimuli such as light and heat. Therefore, materials containing disulfide bonds, like thermoplastic materials, show functions such as repairable processing and shape change. Adding modified conductive filler powder to the conductive silicone rubber system improves the self-healing ability of the conductive silicone rubber; the self-healing of the ester group mainly depends on the ester exchange reaction. Under external stimuli such as heating or mechanical stress, The ester group will break to form new end groups. These end groups diffuse and recombine inside the material to form new ester bonds, thereby filling the damaged area and realizing self-repair of the material, thereby further enhancing the self-repair ability of the conductive silicone rubber. The addition of fluoroalkyl chains can improve the hydrophobicity and surface energy of the modified conductive filler powder, thereby improving the compatibility between acetylene carbon black and other raw materials of conductive silicone rubber, further improving the conductive properties of silicone rubber. At the same time, the good dispersion of the modified conductive filler powder in silicone rubber reduces the agglomeration of acetylene carbon black particles, thereby improving the mechanical properties of silicone rubber.

[0018] Furthermore, the particle size of the acetylene black and the particle size of the graphite are both 70-100 nm, and the particle size of the acetylene black is larger or smaller than the particle size of the graphite.

[0019] By using two conductive filler powders with different particle sizes (acetylene carbon black and graphite), the small-sized conductive filler powder particles can fill the gaps between the large-sized conductive filler powder particles, thereby enhancing the compactness between the conductive filler powder particles, thereby reducing the resistance and improving the conductive properties of the conductive silicone rubber.

[0020] Furthermore, the vulcanization accelerator is zinc oxide.

[0021] Furthermore, the release agent is polytetrafluoroethylene.

[0022] Furthermore, a low-cost preparation process of conductive silicone rubber includes the following steps:

[0023] Methyl vinyl silicone rubber and modified conductive filler powder are put into an internal mixer and mixed for 15-30 minutes. Subsequently, a vulcanization accelerator and a release agent are put into the internal mixer and mixed for 30-50 minutes. The materials in the internal mixer are poured out to obtain low-cost conductive silicone rubber.

[0024] Beneficial effects of the present invention:

[0025] 1. The conductive silicone rubber prepared in the present invention uses modified conductive filler powder as the conductive filler. The main raw materials of the modified conductive filler powder are acetylene carbon black and graphite. These materials have relatively low costs and ensure conductive properties, thereby effectively reducing the overall material cost.

[0026] 2. The conductive silicone rubber produced by the present invention exhibits excellent electrical conductivity, mechanical properties, and self-healing properties. Because conductive silicone rubber contains acetylene black, which has excellent thermal conductivity, existing techniques for producing intrinsically thermally conductive polymers by designing molecular chain structures or adjusting curing networks are extremely difficult. However, the present invention enhances the conductive silicone rubber's ability to self-heal under heating conditions by introducing acetylene black, a material with excellent thermal conductivity. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present invention.

[0028] Example 1

[0029] The preparation method of the modified conductive filling powder of this embodiment is:

[0030] Step A1: Add 24 g of cystine, 80 g of 1H,1H-perfluoro-1-octanol, 2 g of p-toluenesulfonic acid, and 1 L of toluene to a reaction flask and stir; heat to 112° C., reflux for 3 h, cool to -5° C. in a water bath, and keep warm for 1 h; filter with suction, wash with frozen toluene, and dry to obtain a perfluorinated cystine derivative;

[0031] Step A2: 20 g of a perfluorinated cystine derivative was mixed with 4.7 g of KH-560 and reacted at 40° C. for 30 min to obtain a modified silane coupling agent;

[0032] Step A3: Add 3 g of acetylene black, 6 g of graphite, and 0.03 g of modified silane coupling agent to 150 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water is 9:1), stir at 8000 r / min for 20 min, and dry at 80°C for 12 h to obtain modified conductive filler powder.

[0033] The particle size of the acetylene black and the particle size of the graphite are both 70-100 nm, and the particle size of the acetylene black is larger or smaller than that of the graphite.

[0034] Example 2

[0035] The preparation method of the modified conductive filling powder of this embodiment is:

[0036] Step A1: Add 24 g of cystine, 80 g of 1H,1H-perfluoro-1-octanol, 3 g of p-toluenesulfonic acid, and 1.1 L of toluene to a reaction flask and stir; heat to 112° C., reflux for 3 h, cool to 1° C. in a water bath, and keep warm for 1 h; filter with suction, wash with frozen toluene, and dry to obtain a perfluorinated cystine derivative;

[0037] Step A2: 20 g of a perfluorinated cystine derivative was mixed with 4.7 g of KH-560 and reacted at 40° C. for 30 min to obtain a modified silane coupling agent;

[0038] Step A3: Add 4.5 g of acetylene black, 4.5 g of graphite, and 0.04 g of modified silane coupling agent to 150 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water is 9:1), stir at 8000 r / min for 25 min, and dry at 80°C for 12 h to obtain modified conductive filler powder.

[0039] The particle size of the acetylene black and the particle size of the graphite are both 70-100 nm, and the particle size of the acetylene black is larger or smaller than that of the graphite.

[0040] Example 3

[0041] The preparation method of the modified conductive filling powder of this embodiment is:

[0042] Step A1: Add 24 g of cystine, 80 g of 1H,1H-perfluoro-1-octanol, 4 g of p-toluenesulfonic acid, and 1.2 L of toluene to a reaction flask and stir; heat to 112° C., reflux for 3 h, cool to 5° C. in a water bath, and keep warm for 1 h; filter with suction, wash with frozen toluene, and dry to obtain a perfluorinated cystine derivative;

[0043] Step A2: 20 g of a perfluorinated cystine derivative was mixed with 4.7 g of KH-560 and reacted at 40° C. for 30 min to obtain a modified silane coupling agent;

[0044] Step A3: Add 6 g of acetylene black, 3 g of graphite, and 0.06 g of modified silane coupling agent to 150 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water is 9:1), stir at 8000 r / min for 30 min, and dry at 80°C for 12 h to obtain modified conductive filler powder.

[0045] The particle size of the acetylene black and the particle size of the graphite are both 70-100 nm, and the particle size of the acetylene black is larger or smaller than that of the graphite.

[0046] Comparative Example 1

[0047] The preparation method of the modified conductive filling powder of this comparative example is:

[0048] Step A1: Add 24 g of cystine, 20.6 g of trifluoroethanol, 2 g of p-toluenesulfonic acid, and 1 L of toluene to a reaction flask and stir; heat to 106°C, reflux for 3 h, cool to -5°C in a water bath, and keep warm for 1 h; filter, wash with frozen toluene, and dry to obtain a perfluorinated cystine derivative;

[0049] Step A2: 4.1 g of a perfluorinated cystine derivative was mixed with 4.7 g of KH-560 and reacted at 40° C. for 30 min to obtain a modified silane coupling agent;

[0050] Step A3: Add 3 g of acetylene black, 6 g of graphite, and 0.03 g of modified silane coupling agent to 150 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water is 9:1), stir at 8000 r / min for 20 min, and dry at 80°C for 12 h to obtain modified conductive filler powder.

[0051] The particle size of the acetylene black and the particle size of the graphite are both 70-100 nm, and the particle size of the acetylene black is larger or smaller than that of the graphite.

[0052] Comparative Example 2

[0053] The preparation method of the modified conductive filling powder of this comparative example is:

[0054] Step A1: 2.4 g of cystine and 4.7 g of KH-560 were mixed evenly and reacted at 40° C. for 30 min to obtain a modified silane coupling agent;

[0055] Step A2: Add 3 g of acetylene black, 6 g of graphite, and 0.03 g of modified silane coupling agent to 150 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water is 9:1), stir at 8000 r / min for 20 min, and dry at 80°C for 12 h to obtain modified conductive filler powder.

[0056] The particle size of the acetylene black and the particle size of the graphite are both 70-100 nm, and the particle size of the acetylene black is larger or smaller than that of the graphite.

[0057] Comparative Example 3

[0058] The preparation method of the modified conductive filling powder of this comparative example is:

[0059] 3 g of acetylene black, 6 g of graphite, and 0.03 g of KH-560 were added to 150 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water was 9:1), stirred at 8000 r / min for 20 min, and dried at 80° C. for 12 h to obtain a modified conductive filler powder.

[0060] The particle size of the acetylene black and the particle size of the graphite are both 70-100 nm, and the particle size of the acetylene black is larger or smaller than that of the graphite.

[0061] Example 4

[0062] A low-cost conductive silicone rubber comprises the following raw materials in parts by weight: 98 parts of methyl vinyl silicone rubber (molecular weight of 650,000, vinyl molar content of 0.04%), 30 parts of modified conductive filling powder, 2 parts of zinc oxide, and 2 parts of polytetrafluoroethylene.

[0063] This low-cost conductive silicone rubber is made by the following steps:

[0064] Methyl vinyl silicone rubber and conductive filler powder are put into an internal mixer and mixed for 15 minutes. Subsequently, a vulcanization accelerator and a release agent are put into the internal mixer and mixed for 30 minutes. The materials in the internal mixer are poured out to obtain low-cost conductive silicone rubber.

[0065] The preparation steps of the modified conductive filling powder are the same as those in Example 1.

[0066] Example 5

[0067] A low-cost conductive silicone rubber comprises the following raw materials in parts by weight: 96 parts of methyl vinyl silicone rubber (molecular weight of 600,000, vinyl molar content of 0.03%), 40 parts of modified conductive filling powder, 1.5 parts of zinc oxide, and 1.5 parts of polytetrafluoroethylene.

[0068] The molecular weight of the methyl vinyl silicone rubber is 600,000, and the vinyl molar content is 0.03%.

[0069] This low-cost conductive silicone rubber is made by the following steps:

[0070] Methyl vinyl silicone rubber and conductive filler powder are put into an internal mixer and mixed for 20 minutes. Subsequently, a vulcanization accelerator and a release agent are put into the internal mixer and mixed for 40 minutes. The materials in the internal mixer are poured out to obtain low-cost conductive silicone rubber.

[0071] The preparation steps of the modified conductive filler powder are the same as those in Example 2.

[0072] Example 6

[0073] A low-cost conductive silicone rubber comprises the following raw materials in parts by weight: 94 parts of methyl vinyl silicone rubber (molecular weight of 700,000, vinyl molar content of 0.05%), 50 parts of modified conductive filling powder, 1 part of zinc oxide, and 1 part of polytetrafluoroethylene.

[0074] This low-cost conductive silicone rubber is made by the following steps:

[0075] Methyl vinyl silicone rubber and conductive filler powder are put into an internal mixer and mixed for 30 minutes. Subsequently, a vulcanization accelerator and a release agent are put into the internal mixer and mixed for 50 minutes. The materials in the internal mixer are poured out to obtain low-cost conductive silicone rubber.

[0076] The preparation steps of the modified conductive filling powder are the same as those in Example 3.

[0077] Comparative Example 4

[0078] A low-cost conductive silicone rubber is prepared in accordance with Example 4, which differs from Example 4 in that the modified conductive filler powder in Example 4 is replaced by the product prepared in Comparative Example 1, and the remaining raw materials, processes and parameters are the same as those in Example 4.

[0079] Comparative Example 5

[0080] A low-cost conductive silicone rubber is prepared in accordance with Example 4, which differs from Example 4 in that the modified conductive filler powder in Example 4 is replaced by the product prepared in Comparative Example 2, and the remaining raw materials, processes and parameters are the same as those in Example 4.

[0081] Comparative Example 6

[0082] A low-cost conductive silicone rubber is prepared in accordance with Example 4, which differs from Example 4 in that the modified conductive filler powder in Example 4 is replaced by the product prepared in Comparative Example 3, and the remaining raw materials, processes and parameters are the same as those in Example 4.

[0083] The performance of the conductive silicone rubber obtained in Examples 4 to 6 and Comparative Examples 4 to 6 was tested, and the testing process was as follows:

[0084] (1) Resistivity: The volume resistivity of the conductive silicone rubbers prepared in Examples 4 to 6 and Comparative Examples 4 to 6 was measured using a ZC-36 high resistance meter from Shanghai Precision Instrument Co., Ltd. in accordance with the GB / T 1410-2006 test standard.

[0085] (2) Mechanical properties: The conductive silicone rubbers prepared in Examples 4 to 6 and Comparative Examples 4 to 6 were molded into sheets, and the tensile strength and tear strength were tested according to GB / T528-2009.

[0086] (3) Self-healing performance: The dumbbell-shaped sample was cut in the middle and the cut ends were brought into contact with each other. The sample was then transferred to a 100°C oven for 1 h and cooled to room temperature. The tensile strength was tested according to GB / T528-2009. Self-healing rate = tensile strength of the silicone rubber after treatment / tensile strength of the silicone rubber before treatment × 100%.

[0087] Table 1

[0088]

[0089] As can be seen from Table 1, the comprehensive properties of the conductive silicone rubbers prepared in Examples 4 to 6 are better than those prepared in Comparative Examples 6 to 10. The conductive silicone rubber modified conductive filler powder prepared in Comparative Example 6 does not contain long fluorine-containing chains, and its hydrophobicity is lower than that of the thermally conductive silicone rubbers prepared in Examples 4 to 6, thereby affecting the dispersibility of acetylene black and graphite in the silicone rubber, and reducing the mechanical properties and conductive properties of the conductive silicone rubber; the conductive silicone rubber modified conductive filler powder prepared in Comparative Example 7 does not contain fluoroalkyl chains and ester groups, which reduces the dispersibility of acetylene black and graphite in the silicone rubber. At the same time, due to the lack of ester groups, the conductive silicone rubber prepared in this comparative example cannot be ester-repaired. However, the mechanical properties, conductive properties, and self-healing properties of the conductive silicone rubber are reduced compared to the thermally conductive silicone rubber prepared in Examples 4 to 6. The conductive silicone rubber modified conductive filler powder prepared in Comparative Example 7 does not contain fluoroalkyl chains, ester groups, disulfide bonds and other groups, but simply uses a silane coupling agent to silanize acetylene carbon black and graphite. The conductivity and mechanical properties of the conductive silicone rubber are poor. After the conductive silicone rubber is cut in the middle and the sample cuts are brought into contact with each other for thermal repair, no self-healing of the sample is observed.

[0090] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.

[0091] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A low-cost conductive silicone rubber, characterized in that: The invention comprises the following raw materials in parts by weight: 94-98 parts of methyl vinyl silicone rubber, 30-50 parts of modified conductive filling powder, 1-2 parts of vulcanization accelerator and 1-2 parts of release agent.

2. A low-cost conductive silicone rubber according to claim 1, characterized in that: The molecular weight of methyl vinyl silicone rubber is 600,000-700,000, and the molar content of vinyl is 0.03%-0.05%.

3. A low-cost conductive silicone rubber according to claim 1, characterized in that: The preparation method of the modified conductive filling powder is as follows: Step A1: Add cystine, 1H,1H-perfluoro-1-octanol, p-toluenesulfonic acid and toluene into a reaction flask and stir; Raise the temperature to 112°C, keep the temperature under reflux for 3 hours, cool to -5 to 5°C, keep the temperature for 1 hour; filter, wash, and dry to obtain a perfluorinated derivative of cystine; Step A2: Mix the perfluorinated derivative of cystine with KH-560 and react at 40° C. for 30 min to obtain a modified silane coupling agent; Step A3: Add acetylene carbon black, graphite and modified silane coupling agent into ethanol aqueous solution, stir at 8000 r / min for 20-30 min, and dry at 80° C. for 12 h to obtain modified conductive filling powder.

4. A low-cost conductive silicone rubber according to claim 3, characterized in that: In step A1, the usage ratio of cystine, 1H,1H-perfluoro-1-octanol, p-toluenesulfonic acid and toluene is 24 g:80 g:2-4 g:1-1.2 L.

5. A low-cost conductive silicone rubber according to claim 3, characterized in that: In step A2, the mass ratio of the perfluorinated derivative of cystine to KH-560 is 20:4.

7.

6. A low-cost conductive silicone rubber according to claim 3, characterized in that: In step A3, the usage ratio of acetylene carbon black, graphite, modified silane coupling agent and ethanol aqueous solution is 3-6 g: 3-6 g: 0.03-0.06 g: 150 mL; the volume ratio of anhydrous ethanol and deionized water in the ethanol aqueous solution is 9:

1.

7. A low-cost conductive silicone rubber according to claim 3, characterized in that: In step A3, the particle size of acetylene black and the particle size of graphite are both 70-100 nm, and the particle size of acetylene black is larger or smaller than the particle size of graphite.

8. The low-cost conductive silicone rubber according to claim 1, characterized in that: The vulcanization accelerator is zinc oxide.

9. The low-cost conductive silicone rubber according to claim 1, characterized in that: The release agent is polytetrafluoroethylene.

10. A process for preparing low-cost conductive silicone rubber according to any one of claims 1 to 9, characterized in that: The following steps are involved: Put methyl vinyl silicone rubber and modified conductive filler powder into an internal mixer and mix for 15-30 minutes. Then put vulcanization accelerator and release agent into the internal mixer and mix for 30-50 minutes. Pour out the materials in the internal mixer to obtain low-cost conductive silicone rubber.

Citation Information

Patent Citations

  • A conductive silicone rubber with low tensile permanent deformation and its preparation method

    CN112210215B

Cited By

  • Preparation method of conductive silicone rubber base material for anti-pinch door

    CN122854806A