High-transparency gamma-quinacridone organic pigment and preparation method thereof
By performing a closed-loop reaction in the presence of polyphosphoric acid and reflux treatment with additives, the problem of uneven distribution of the particle size of γ-type quinacridone organic pigment was solved, and a highly transparent γ-type quinacridone was prepared. Organic pigments extend their use range in a variety of industrial applications.
Patent Information
- Application Number
- CN202411175201.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The particle size distribution of existing γ-type quinacridone organic pigments is uneven, resulting in insufficient transparency, limiting its application.
Prepare α-type quinacridone crude product by performing closed-loop reaction in the presence of polyphosphoric acid, and reflux treatment is used with specific additives to convert it into a small particle size γ-type quinacridone organic pigment to improve its transparency .
The high transparency of the γ-type quinacridone organic pigment is achieved, with a particle size of 0.03 to 0.1 μm, which improves its application performance in coatings, inks, plastic products and textile fiber slurries.
Smart Images

Figure CN119060558A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pigment chemical industry, in particular to a method for preparing a high-transparency gamma-quinacridone organic pigment. Background Art
[0002] Organic pigments play an important role in modern industry with their excellent color expression and chemical stability. γ-quinacridone, as a special organic pigment, exhibits excellent color vividness and various application fastness with its unique chemical structure and molecular arrangement. However, the particle size distribution of γ-quinacridone prepared by ordinary methods is uneven, or the particles are too large, and the transparency is insufficient during the application process, which limits the specific application occasions of γ-quinacridone. Summary of the invention
[0003] 1. Technical issues to be solved
[0004] In view of the state of the prior art, the present invention provides a method for preparing a highly transparent γ-quinacridone organic pigment, which solves the problems raised in the above-mentioned background technology by regulating the preparation temperature and specific pigmentation treatment.
[0005] (II) Technical solution
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] According to a first aspect of the present invention, there is provided a method for preparing a highly transparent γ-type quinacridone organic pigment, comprising the following steps:
[0008] (1) In the presence of polyphosphoric acid, 2,5-diphenylaminoterephthalic acid undergoes a ring-closing reaction at 135-140° C. to obtain a crude α-quinacridone;
[0009] (2) diluting the α-quinacridone crude product with water and filtering the obtained filter cake, and then refluxing it in an organic solvent containing an auxiliary agent to obtain a γ-quinacridone organic pigment with high transparency;
[0010] Wherein, the auxiliary agent is selected from at least one of a lipophilic surfactant or a derivative of a quinacridone parent structure.
[0011] The reaction formula for preparing the crude α-quinacridone product shown in Formula II in step (1) of the present invention is as follows:
[0012]
[0013] The present invention can obtain more α-quinacridone crude products with smaller particle sizes by reacting at 135-140° C., and then through the specific pigmentation treatment in step (2), a specific auxiliary agent is selected to refine the particles of the α-quinacridone crude product and transform the crystal form to obtain a γ-quinacridone organic pigment with smaller particle size. During the application process, a γ-quinacridone organic pigment with high transparency can be obtained.
[0014] Specifically, the lipophilic surfactant of the present invention is selected from rosin amine, hydrogenated rosin amine, disproportionated rosin amine, adducts prepared by the reaction of alkylphenol or fatty alcohol with ethylene oxide, OP series of polyoxyethylene alkylphenol condensates, Perepend O series of polyoxyethylene fatty alcohol condensates, Tween series of polyoxyethylene polyol ether fatty acid esters, and ethylene oxide adduct series of fatty amines.
[0015] The structural formula of the derivative of the quinacridone parent structure is as follows:
[0016]
[0017] Wherein R1 and R2 are selected from H, -COOH, -CONHR, -CH2NHCOR, -SO3H, At least one of .
[0018] Preferably, in step (1), the concentration of the polyphosphoric acid is 100-105%.
[0019] Optionally, in step (1), the concentration of the polyphosphoric acid is selected from any value of 100%, 101%, 102%, 103%, 104%, 105%, or a range between any two values.
[0020] Preferably, in step (2), the organic solvent is selected from any one of methanol, ethanol, isobutanol, dimethylformamide or acetic acid.
[0021] Preferably, in step (2), the amount of the organic solvent used is 12 to 14 times that of the crude α-quinacridone.
[0022] Preferably, in step (2), the amount of the auxiliary agent used is 0.5-5% of the crude α-quinacridone.
[0023] Preferably, in step (2), the reflux treatment time is 2 to 4 hours.
[0024] Optionally, in step (2), the reflux treatment time is selected from any value among 2h, 3h, 4h or a range between any two values.
[0025] It should be noted that the reflux temperature in the present invention is the boiling point of the organic solvent used.
[0026] According to a second aspect of the present invention, a highly transparent γ-quinacridone organic pigment is obtained according to the above preparation method, wherein the particle size of the γ-quinacridone organic pigment is 0.03-0.1 μm.
[0027] (III) Beneficial effects
[0028] The present invention provides a highly transparent γ-type quinacridone organic pigment and a preparation method thereof. The pigment has the following beneficial effects:
[0029] (1) The present invention provides a method for preparing a highly transparent γ-quinacridone organic pigment. By precisely controlling the reaction temperature, a pure α-quinacridone crude product is prepared. After a specific pigmentation treatment and the selection of specific additives, the α-quinacridone crude product has a pigment particle size of less than 0.1 μm and is converted into a γ-quinacridone. Thus, the crude product exhibits extremely high tinting strength and transparency during application.
[0030] (2) The present invention provides a method for preparing a highly transparent γ-quinacridone organic pigment. By controlling the concentration of polyphosphoric acid, not only the reaction rate can be controlled, but also a high-purity α-quinacridone crude product can be generated, and the conversion rate is further improved.
[0031] (3) This scheme provides a highly transparent γ-type quinacridone organic pigment with a particle size range of 0.03 to 0.1 μm. It has excellent color expression and transparency and can be used not only in traditional coatings and inks, but also in the fields of high-end plastic products and textile fiber pulp coloring. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the X-ray powder diffraction curve of the γ-quinacridone organic pigment prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0033] In order to better illustrate the content of the present invention, a detailed description is given below in conjunction with specific embodiments.
[0034] Example 1
[0035] 1000 g of 2,5-diphenylamino terephthalic acid was added to a polyphosphoric acid solution with a concentration of 100%, and a ring-closing reaction was carried out at 135° C. The α-quinacridone crude product cake was obtained after dilution with water and filtration;
[0036] 4.48 g of rosin amine was dissolved in 10.74 kg of methanol and mixed evenly to obtain a mixed solution. The α-quinacridone crude filter cake was added to the mixed solution and refluxed at 67° C. for 2 h to obtain a γ-quinacridone organic pigment with a particle size of 0.03 to 0.1 μm, such as Figure 1 shown.
[0037] Example 2
[0038] 1000 g of 2,5-diphenylamino terephthalic acid was added to a polyphosphoric acid solution having a concentration of 105%, and a ring-closing reaction occurred at 137° C. The α-quinacridone crude product filter cake was obtained after dilution with water and filtration;
[0039] 8.9 g of hydrogenated rosin amine was dissolved in 11.75 kg of ethanol and mixed evenly to obtain a mixed solution. The α-quinacridone crude filter cake was added to the mixed solution and refluxed at 78° C. for 3 h to obtain a γ-quinacridone organic pigment with a particle size of 0.03 to 0.1 μm.
[0040] Example 3
[0041] 1000 g of 2,5-diphenylamino terephthalic acid was added to a polyphosphoric acid solution with a concentration of 103%, and a ring-closing reaction was carried out at 140° C. The α-quinacridone crude product filter cake was obtained after dilution with water and filtration;
[0042] 26.85 g of disproportionated rosin amine was dissolved in 12.53 kg of isobutyl alcohol and mixed evenly to obtain a mixed solution. The α-quinacridone crude filter cake was added to the mixed solution and refluxed at 108° C. for 4 hours to obtain a γ-quinacridone organic pigment with a particle size of 0.03 to 0.1 μm.
[0043] Example 4
[0044] The preparation method of this embodiment is the same as that of embodiment 1, except that the selected organic solvent is dimethylformamide, and after refluxing, a γ-type quinacridone organic pigment with a particle size of 0.03 to 0.1 μm is obtained.
[0045] Example 5
[0046] The preparation method of this embodiment is the same as that of embodiment 1, except that the selected organic solvent is acetic acid, and after refluxing, a γ-type quinacridone organic pigment with a particle size of 0.03 to 0.1 μm is obtained.
[0047] The invention prepares a gamma-quinacridone organic pigment with a particle size range of 0.03 to 0.1 μm by regulating the concentration of polyphosphoric acid, the closed-loop reaction time, the addition of an auxiliary agent and the reflux time. During the application process, the pigment has excellent transparency and extremely high tinting strength.
[0048] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a highly transparent γ-quinacridone organic pigment, characterized in that: The following steps are involved: (1) In the presence of polyphosphoric acid, 2,5-diphenylaminoterephthalic acid undergoes a ring-closing reaction at 135-140° C. to obtain a crude α-quinacridone; (2) diluting the α-quinacridone crude product with water and filtering it, and then refluxing the obtained filter cake in an organic solvent containing an auxiliary agent to obtain a γ-quinacridone organic pigment with high transparency; Wherein, the auxiliary agent is selected from at least one of a lipophilic surfactant or a derivative of a quinacridone parent structure.
2. The method for preparing a highly transparent γ-quinacridone organic pigment according to claim 1, characterized in that: In step (1), the concentration of the polyphosphoric acid is 100-105%.
3. The method for preparing a highly transparent γ-quinacridone organic pigment according to claim 1, characterized in that: In step (2), the organic solvent is selected from any one of methanol, ethanol, isobutanol, dimethylformamide or acetic acid.
4. The method for preparing a highly transparent γ-quinacridone organic pigment according to claim 1, characterized in that: In step (2), the amount of the organic solvent used is 12 to 14 times that of the crude α-quinacridone.
5. The method for preparing a highly transparent γ-quinacridone organic pigment according to claim 1, characterized in that: In step (2), the amount of the auxiliary agent used is 0.5-5% of the crude α-quinacridone.
6. The method for preparing a highly transparent γ-quinacridone organic pigment according to claim 1, characterized in that: In step (2), the reflux treatment time is 2 to 4 hours.
7. A highly transparent γ-type quinacridone organic pigment obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The particle size of the γ-type quinacridone organic pigment is 0.03-0.1 μm.
Citation Information
Patent Citations
A class of Quinacridone polyether derivatives, preparation method and applications thereof
CN107057054A
Method for producing quinacridone pigment
CN112110915A
Production process of quinacridone pigment
CN113652098A
Production process of quinacridone pigment
CN116239894A
Preparation technology for quinacridone organic pigment
CN1229107A