High-oil-absorption iron oxide red with amphiphilic transparent surface and preparation method of high-oil-absorption iron oxide red
By covering SiO2 and Al2O3 films on the surface of the iron red powder, the oil absorption of iron red pigments is improved, and the problem of insufficient oil absorption of existing iron red pigments is solved, and the preparation of high oil absorption of iron red is achieved, which is suitable for large-scale production And keep the original color.
Patent Information
- Application Number
- CN202411303629.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
The existing iron red pigment has a low oil absorption capacity and is difficult to use in matte coatings. There are fewer methods for preparing iron red with high oil absorption capacity, which limits its application range.
By uniformly covering the transparent film, SiO2 film and Al2O3 film on the surface of the iron red powder, the coating is sequentially from the inside to the outside, the oil absorption is increased, and a simple preparation method is adopted to suit large-scale production.
It has achieved high oil absorption of iron red pigments, maintained the original color, and is suitable for large-scale production, which has significantly improved the oil absorption performance of iron red powder.
Smart Images

Figure CN119060563A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coating preparation, and particularly relates to an iron red with an amphiphilic transparent surface and high oil absorption and a preparation method thereof. Background Art
[0002] Iron oxide (Fe2O3) is a high-grade pigment widely used in high-end automotive coatings, architectural coatings, anti-corrosion coatings, powder coatings and other fields. The annual consumption worldwide exceeds 1 million tons, second only to titanium dioxide and ranking second among inorganic pigments. Using iron oxide as a pigment not only maintains the good heat resistance, weather resistance and ultraviolet absorption advantages of general inorganic pigments, but also can be well dispersed in oily carriers. The coatings or inks prepared with it have satisfactory transparency. At the same time, different oil absorption is of great significance to the production of oily pigments and the connection of pigment layers. Matt coatings tend to have high oil absorption of pigments, while glossy coatings tend to have low oil absorption of pigments. Ordinary iron oxide red pigments have low oil absorption, so it is difficult to use as matte coatings. In order to expand the application range of iron oxide red and increase its oil absorption, it is an effective method to modify its surface by aluminum oxide coating. The aluminum oxide aluminum coating layer is lipophilic, and due to the loose surface, the oil absorption area of iron oxide red can be increased, thereby improving the oil absorption performance of iron oxide red pigment. However, it is difficult to directly coat alumina on the surface of iron red. In existing research, there are still few reports on the preparation method of iron red with high oil absorption. Developing a preparation method of iron red pigment with high oil absorption is of great practical significance. Summary of the invention
[0003] One of the purposes of the present invention is to provide an iron oxide with high oil absorption and an amphiphilic transparent surface, which is coated with a transparent film and can increase the oil absorption of the iron oxide without changing the color of the iron oxide itself.
[0004] The second object of the present invention is to provide a method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface, which is simple to operate, low in cost and suitable for large-scale production and application.
[0005] The technical solution provided by the present invention is:
[0006] The invention discloses an iron red with high oil absorption and an amphiphilic transparent surface. The outer surface of the iron red powder is uniformly coated with a transparent film, and the transparent film is a SiO2 film and an Al2O3 film from the inside to the outside.
[0007] Preferably, the theoretical coating amount of the SiO2 film is 2wt%, and the theoretical coating amount of the Al2O3 film is 0.5wt%-2.5wt%.
[0008] A method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface, which is used to prepare iron oxide red with high oil absorption and having an amphiphilic transparent surface as claimed in the claims, comprises the following steps:
[0009] Step 1: Add iron oxide red powder and dispersant into deionized water, heat and stir, adjust the pH value to 8-8.5, and continue to disperse to obtain a dispersed system;
[0010] Step 2, maintaining the temperature of the dispersion system at 50°C-90°C, adjusting the pH value to 9-12, adding SiO2 precursor solution for SiO2 coating, and then adding Al2O3 precursor solution for Al2O3 coating;
[0011] Among them, the pH value is maintained at 9-12 during the coating process;
[0012] Step 3, subjecting the reaction system after the coating treatment to aging treatment;
[0013] Step 4: After filtering, washing and drying the aged reaction system, iron red with an amphiphilic transparent surface and high oil absorption is obtained.
[0014] Preferably, in step 1, the mass ratio of iron ore red powder to deionized water is 1:2-1:6.
[0015] Preferably, the dispersant is sodium hexametaphosphate, sodium tripolyphosphate, sodium pyrophosphate or sodium citrate, and the mass ratio of the dispersant to deionized water is 1:400-1:600.
[0016] Preferably, in step 1, the dispersion stirring rate is 200 r / min-300 r / min, and the dispersion time is 40 min.
[0017] Preferably, in step 2, the coating treatment method is:
[0018] The SiO2 precursor solution is added at a uniform speed and stirred continuously for SiO2 coating. The SiO2 precursor solution is added for 60 minutes. After SiO2 coating, it is stirred for 10 minutes. Then, the Al2O3 precursor solution is added at a uniform speed and stirred continuously for Al2O3 coating. The Al2O3 precursor solution is added for 15 minutes to 75 minutes.
[0019] Preferably, the SiO2 precursor solution is a soluble silicate solution; the mass concentration of the SiO2 precursor solution is 10% based on SiO2;
[0020] The Al2O3 precursor solution is a soluble aluminate solution; the mass concentration of the Al2O3 precursor solution is 10% based on Al2O3.
[0021] Preferably, in the step three, the pH value of the reaction system after the coating treatment is adjusted to 7-7.5, and the aging treatment is performed at 50° C.-90° C. for 30 minutes.
[0022] Preferably, in step 4, after filtering the aged reaction system, deionized water is added for washing until the conductivity of the washing water is less than 200 μS / cm; and the filter cake obtained by washing is dried at a temperature of 160° C.-200° C. for 3 h-5 h.
[0023] The beneficial effects of the present invention are:
[0024] The iron red with high oil absorption and amphiphilic transparent surface provided by the invention is coated with a transparent film, which can improve the oil absorption of the iron red and will not change the color of the iron red itself.
[0025] The method for preparing the iron oxide red with an amphiphilic transparent surface and high oil absorption provided by the invention has the advantages of simple operation, low cost and suitability for large-scale production and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a comparison chart of the oil absorption of the high oil absorption iron oxide prepared in Example 4 of the present invention and the commercially available iron oxide product.
[0027] Figure 2 This is a graph showing the oil absorption test results of the high oil absorption iron oxide prepared in Examples 1-5 of the present invention.
[0028] Figure 3 The oil absorption test results of the high oil absorption iron oxide prepared in Examples 4, 6-10 of the present invention.
[0029] Figure 4 This is a scanning electron microscope (SEM) photograph of commercially available iron red powder.
[0030] Figure 5 (a) is a scanning electron microscope (SEM) photograph of the high oil absorption iron oxide prepared in Example 4 of the present invention.
[0031] Figure 5 (b) is the DSmapping spectrum of the high oil absorption iron oxide prepared in Example 4 of the present invention.
[0032] Figure 6 This is the appearance of commercially available iron red powder.
[0033] Figure 7 This is the appearance of the iron red powder with high oil absorption prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0035] The invention provides a high oil absorption iron oxide with an amphiphilic transparent surface, wherein a transparent film is uniformly coated on the outer surface of the iron oxide powder, and the transparent film is a SiO2 film and an Al2O3 film from the inside to the outside. The mass of the added SiO2 precursor makes the mass ratio of SiO2 to the iron oxide powder 1:50, and the theoretical coating amount of the SiO2 film is 2wt%, and the mass of the added Al2O3 precursor makes the mass ratio of Al2O3 to the iron oxide powder 1:40-1:200, and the theoretical coating amount of the Al2O3 film is 0.5wt%-2.5wt%. The theoretical coating amount of the SiO2 film refers to the mass ratio of SiO2 to the (uncoated) iron oxide powder; the theoretical coating amount of the Al2O3 film refers to the mass ratio of Al2O3 to the (uncoated) iron oxide powder.
[0036] As a further preference, the theoretical coating amount of the Al2O3 film is 2 wt%.
[0037] The present invention also provides a method for preparing the iron oxide red with high oil absorption having an amphiphilic transparent surface, which is used to prepare the iron oxide red with high oil absorption having an amphiphilic transparent surface. The specific preparation process is as follows.
[0038] 1. Dispersion: Add iron oxide red powder to deionized water, add dispersant, heat and stir to 50℃-90℃, adjust pH value to 8-8.5, and continue to disperse to obtain a dispersed system.
[0039] The mass ratio of iron ore red powder to deionized water is 1:2-1:6; the composition of iron ore red powder is Fe2O3, and the average particle size is between 0.1 μm and 1 μm.
[0040] Preferably, the dispersant is sodium hexametaphosphate, sodium tripolyphosphate, sodium pyrophosphate or sodium citrate, and the mass ratio of the added amount of the dispersant to the deionized water is 1:400-1:600.
[0041] Preferably, the dispersion stirring rate is set to 200 r / min-300 r / min, and the dispersion time is 40 min.
[0042] 2. Coating treatment. Maintain the temperature of the dispersed system at 50°C-90°C, adjust the pH value to 9-12, uniformly add a SiO2 precursor solution with a theoretical SiO2 coating amount of 2wt% and continue stirring for coating treatment. After the SiO2 coating is completed, maintain the temperature of the dispersed system at 50°C-90°C, adjust the pH value to 9-12, stir for 10 minutes, uniformly add an Al2O3 precursor solution with a theoretical Al2O3 coating amount of 0.5wt%-2.5wt% and continue stirring for coating treatment.
[0043] Wherein, the SiO2 precursor solution adopts a soluble silicate solution.
[0044] Preferably, the SiO2 precursor solution is Na2SiO3 or K2SiO3 solution, with a mass concentration of 10% (in terms of SiO2). The SiO2 precursor solution is added for 60 minutes.
[0045] During the coating process, 10 wt% sulfuric acid and 10 wt% sodium hydroxide were used to maintain the pH at 9-12.
[0046] The Al2O3 driving body solution adopts a soluble aluminate solution.
[0047] Preferably, the Al2O3 precursor solution is a NaAlO2 solution with a mass concentration of 10% (calculated as Al2O3). The Al2O3 precursor solution is added for 15 min to 75 min.
[0048] During the coating treatment, 10 wt % sulfuric acid and 10 wt % sodium hydroxide were used to maintain the pH at 9-12.
[0049] 3. Aging treatment: Adjust the pH value of the reaction system after coating treatment to 7-7.5, and perform aging treatment at 50℃-90℃; the aging treatment time is 30 minutes, and stirring is continued during the aging process.
[0050] 4. Filtration and drying: Filter the system after aging treatment, add deionized water for washing until the conductivity of the washing water is less than 200μS / cm, and dry the filter cake obtained after washing at 160℃-200℃ for 3-5h to obtain iron red with high oil absorption.
[0051] Example 1
[0052] (1) Take 50g of iron ore red powder and add it to 200ml of deionized water, then add 0.4g of sodium hexametaphosphate;
[0053] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 75° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0054] (3) After the dispersion is completed, the pH is adjusted to 10.5-11, and 10 ml of 10 wt% Na2SiO3 is added at a uniform rate within 60 minutes and stirred continuously for coating. After the silicon coating is completed, stir for 10 minutes, and then 2.5 ml of 10 wt% NaAlO2 is added at a uniform rate within 15 minutes and stirred continuously for coating. During this period, 10 wt% H2SO4 and 10 wt% NaOH are used to maintain the pH at 10.5-11.
[0055] (4) After the coating is completed, stirring is continued for 30 minutes, and the pH value is adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 minutes, during which the pH is maintained at 7-7.5.
[0056] The stirring speed during the coating and aging process was 260 r / min.
[0057] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0058] Example 2
[0059] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0060] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 50° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0061] (3) After the dispersion is completed, the pH is adjusted to 10.5-11, and 10 ml of 10 wt% Na2SiO3 is added at a uniform rate within 60 minutes and stirred continuously for coating. After the silicon coating is completed, stir for 10 minutes, and then 5 ml of 10 wt% NaAlO2 is added at a uniform rate within 30 minutes and stirred continuously for coating. During this period, 10 wt% H2SO4 and 10 wt% NaOH are used to maintain the pH at 10.5-11.
[0062] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0063] The stirring speed during the coating and aging process was 260 r / min.
[0064] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0065] Example 3
[0066] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0067] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 90° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0068] (3) After the dispersion is completed, the pH is adjusted to 10.5-11, and 10 ml of 10 wt% Na2SiO3 is added at a uniform rate within 60 minutes and stirred continuously for coating. After the silicon coating is completed, stir for 10 minutes, and then 7.5 ml of 10 wt% NaAlO2 is added at a uniform rate within 45 minutes and stirred continuously for coating. During this period, 10 wt% H2SO4 and 10 wt% NaOH are used to maintain the pH at 10.5-11.
[0069] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0070] The stirring speed during the coating and aging process was 260 r / min.
[0071] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0072] Example 4
[0073] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0074] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 75° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0075] (3) After the dispersion is completed, the pH is adjusted to 10.5-11, and 10 ml of 10 wt% Na2SiO3 is added at a uniform rate within 60 minutes and stirred continuously for coating. After the silicon coating is completed, stir for 10 minutes, and then 10 ml of 10 wt% NaAlO2 is added at a uniform rate within 60 minutes and stirred continuously for coating. During this period, 10 wt% H2SO4 and 10 wt% NaOH are used to maintain the pH at 10.5-11.
[0076] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0077] The stirring speed during the coating and aging process was 260 r / min.
[0078] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0079] Example 5
[0080] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0081] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 75° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0082] (3) After the dispersion is completed, the pH is adjusted to 10.5-11, and 10 ml of 10 wt% Na2SiO3 is added at a uniform rate within 60 minutes and stirred continuously for coating. After the silicon coating is completed, stir for 10 minutes, and then 12.5 ml of 10 wt% NaAlO2 is added at a uniform rate within 75 minutes and stirred continuously for coating. During this period, 10 wt% H2SO4 and 10 wt% NaOH are used to maintain the pH at 10.5-11.
[0083] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0084] The stirring speed during the coating and aging process was 260 r / min.
[0085] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0086] Example 6
[0087] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0088] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 75° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0089] (3) After dispersion, adjust the pH to 9-9.5, add 10 ml of 10 wt% Na2SiO3 at a constant speed within 60 min and continue to stir for coating. After silicon coating, stir for 10 min, then add 10 ml of 10 wt% NaAlO2 at a constant speed within 60 min and continue to stir for coating. During this period, use 10 wt% sulfuric acid and 10 wt% NaOH to maintain the pH at 9-9.5.
[0090] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0091] The stirring speed during the coating and aging process was 260 r / min.
[0092] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0093] Example 7
[0094] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0095] (2) starting a water bath and a stirrer, adjusting the stirrer speed to 260 r / min, suspending the solid particles in water, heating to 75° C., adjusting the pH to 8-8.5 using 10 wt % NaOH, and dispersing for 40 min;
[0096] (3) After dispersion, adjust the pH to 9.5-10, add 10 ml of 10 wt% Na2SiO3 at a constant speed within 60 min and continue to stir for coating. After silicon coating, stir for 10 min, then add 10 ml of 10 wt% NaAlO2 at a constant speed within 60 min and continue to stir for coating. During this period, use 10 wt% H2SO4 and 10 wt% NaOH to maintain the pH at 9.5-10.
[0097] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0098] The stirring speed during the coating and aging process was 260 r / min.
[0099] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0100] Example 8
[0101] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0102] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 75° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0103] (3) After dispersion, adjust the pH to 10-10.5, add 10 ml of 10 wt% Na2SiO3 at a constant speed within 60 min and continue to stir for coating. After coating, stir for 10 min, then add 10 ml of 10 wt% NaAlO2 at a constant speed within 60 min and continue to stir for coating. During this period, use 10 wt% H2SO4 and 10 wt% NaOH to maintain the pH at 10-10.5.
[0104] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0105] The stirring speed during the coating and aging process was 260 r / min.
[0106] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0107] Example 9
[0108] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0109] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 75° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0110] (3) After dispersion, adjust the pH to 11-11.5, add 10 ml of 10 wt% Na2SiO3 at a constant speed within 60 min and continue to stir for coating. After coating, stir for 10 min, then add 10 ml of 10 wt% NaAlO2 at a constant speed within 60 min and continue to stir for coating. During this period, use 10 wt% H2SO4 and 10 wt% NaOH to maintain the pH at 11-11.5.
[0111] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0112] The stirring speed during the coating and aging process was 260 r / min.
[0113] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0114] Example 10
[0115] (1) Take 50 g of iron ore red powder and add it to 200 ml of deionized water, and then add 0.4 g of sodium hexametaphosphate.
[0116] (2) Start the water bath and stirrer, adjust the stirrer speed to 260 r / min, suspend the solid particles in water, heat to 75° C., use 10 wt % NaOH to adjust the pH to 8-8.5, and disperse for 40 min.
[0117] (3) After dispersion, adjust the pH to 11.5-12, add 10 ml of 10 wt% Na2SiO3 at a constant speed within 60 min and continue to stir for coating. After silicon coating, stir for 10 min, then add 10 ml of 10 wt% NaAlO2 at a constant speed within 60 min and continue to stir for coating. During this period, use 10 wt% H2SO4 and 10 wt% NaOH to maintain the pH at 11.5-12.
[0118] (4) After coating, stirring was continued for 30 min, and the pH value was adjusted to 7-7.5 using 10 wt% H2SO4, and aged for 30 min, during which the pH was maintained at 7-7.5.
[0119] The stirring speed during the coating and aging process was 260 r / min.
[0120] (5) After aging, the solid was filtered out, washed with deionized water until the conductivity was less than 200 μS / cm, dried at 180° C., ground and bagged.
[0121] Test example
[0122] Take 5g of each of the high oil absorption iron red sample powders obtained in Examples 1-10 and 5g of commercially available iron red powder, place them in a glass evaporating dish, drop refined linseed oil, and mix them evenly with a palette knife. When a uniform paste is formed that is just not cracked or broken and can be scooped up with a palette knife, the end point is reached. At this time, record the amount of refined linseed oil used, and convert it to the oil absorption of 100g of the sample to be tested and make a record. The oil absorption test results of each embodiment are shown in Table 1. The experimental results are compared. Figure 1 , Figure 2 and Figure 3 shown.
[0123] Table 1 Oil absorption test results of each embodiment
[0124]
[0125]
[0126] As shown in Table 1, the oil absorption of the high oil absorption iron oxide red prepared in Examples 1-10 is all above 61.5 g / 100 g, which is higher than the oil absorption of commercially available iron oxide red.
[0127] like Figure 1 As shown, the oil absorption of commercially available iron oxide red is 48 g / 100 g. After being coated and modified by Example 4, the oil absorption of the sample powder is 68.5 g / 100 g, which is significantly improved compared with the oil absorption of the uncoated iron oxide red.
[0128] This proves that the coating materials are attached to the powder, changing the surface properties of the iron red powder. Compared with ordinary iron red powder, the oil absorption of the sample modified by silica-alumina coating obtained in Example 4 is greatly improved, and the modification has achieved remarkable results.
[0129] By comparing Examples 1-5, the effect of the amount of alumina coating on the oil absorption can be observed, such as Figure 2 As shown in Figure 2, as the theoretical coating amount of Al2O3 increases from 0.5wt% to 2.5wt%, the oil absorption of the iron red powder gradually increases, reaching a maximum value at 2wt% and then decreasing.
[0130] This is because when the coating amount is small, the aluminum oxide layer coated on the surface of the iron red powder is thinner and the oleophilic surface is smaller, resulting in less oil absorption than the powder with a larger aluminum coating amount. The oil absorption of the iron red powder with a theoretical coating amount of 2wt% is similar to that of the theoretical coating amount of 2.5wt%, and the oil absorption of the theoretical coating amount of 2.5wt% is slightly smaller in comparison, indicating that the coating effect is best when the theoretical coating amount is 2wt%, and the coating surface is the most complete, which increases the specific surface area of the iron red powder and increases the oil absorption; when the coating amount is increased further, the distance between the iron red particles is reduced due to excessive coating, the specific surface area is reduced, the oil absorption is reduced, and the cost is increased. Therefore, the actual coating amount of aluminum oxide should be adjusted according to the actual application needs.
[0131] By comparing the oil absorption of Example 4 and Examples 6-10, it can be observed that the pH value of the coating process affects the oil absorption of the sample coated by the method, such as Figure 3 As shown in the figure, with the continuous increase of pH value, the oil absorption of the sample shows an overall trend of first increasing and then decreasing. During the coating process, the oil absorption is the highest when the pH value is 10.5-11, and the coating effect is the most ideal. Lower or higher pH values will reduce the oil absorption.
[0132] This is because the pH value of the coating is too low, the hydrolysis rate of NaAlO2 is too fast, and its solution undergoes homogeneous nucleation, resulting in Al2O3 self-aggregating and precipitating before being coated on the surface of the iron ore red powder, reducing the Al2O3 coating amount on the surface of the iron ore red powder and the oil absorption of the iron ore red powder; if the pH value of the coating is too high, it will inhibit the occurrence of the NaAlO2 hydrolysis reaction, causing NaAlO2 to hydrolyze less or not hydrolyze, and then it cannot be hydrolyzed into Al2O3 to be coated on the surface of the iron ore red powder, resulting in a reduction in the coating amount, and then reducing its oil absorption.
[0133] The effect of silicon oxide-aluminum oxide coating on the morphology of red iron powder was analyzed by scanning electron microscopy (SEM) combined with EDS energy spectrometer, and the morphology of the micro-area was observed and the composition of the micro-area was analyzed.
[0134] The SEM images of the commercially available iron red powder and the sample powder obtained in Example 4 are shown in the following figure: Figure 4 and Figure 5 As shown in (a). The shape and particle size distribution of commercially available iron red are uneven, among which the larger ones are about 500nm and the smaller ones are less than 100nm. Most of them exist in the form of agglomerates. The average particle size of 1μm detected is obviously also derived from the agglomerates. Compared with Fe2O3, the powder morphology obtained in Example 4 of the present invention has no significant change in the overall morphology, the edges are relatively smooth, and there are a small number of agglomerated small particles, indicating the existence of a coating layer. Figure 5 As shown in (b), EDS mapping analysis shows that the Fe, O, Si and Al elements of Example 4 are well distributed in the particles, and the Si and Al elements are spread throughout the entire figure, which once again proves the existence and uniform coating of the SiO2 and Al2O3 coating layers. From the distribution position, it can be seen that the content of Si and Al elements is significantly lower than that of Fe and O elements, which also proves that SiO2 is a very thin coating on the outer layer of Fe2O3.
[0135] Appearance: Commercially available iron red powder (such as Figure 6 ) and a photograph of the sample powder prepared in Example 4 of the present invention (as shown Figure 7 As shown), it can be seen that the silicon oxide-aluminum oxide film coated on the surface of the iron ore red powder is a transparent film, and the appearance color of the sample obtained in the embodiment of the present invention has no significant difference from the original commercially available iron ore red powder.
[0136] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A high oil absorption iron red having an amphiphilic transparent surface, characterized in that: The outer surface of the iron ore powder is uniformly covered with a transparent film, and the transparent film is a SiO2 film and an Al2O3 film from the inside to the outside.
2. The iron red with high oil absorption having an amphiphilic transparent surface according to claim 1, characterized in that: The coating amount of the SiO2 film is 2wt%, and the coating amount of the Al2O3 film is 0.5wt%-2.5wt%.
3. A method for preparing iron red with high oil absorption having an amphiphilic transparent surface, characterized in that: The method for preparing the iron red with high oil absorption and having an amphiphilic transparent surface as claimed in any one of claims 1 or 2 comprises the following steps: Step 1: Add iron red powder and dispersant into deionized water, heat and stir, and adjust the pH value to 8- 8.5, continue to disperse to obtain a dispersed system; Step 2, maintaining the temperature of the dispersion system at 50°C-90°C, adjusting the pH value to 9-12, adding SiO2 precursor solution for SiO2 coating, and then adding Al2O3 precursor solution for Al2O3 coating; Among them, the pH value is maintained at 9-12 during the coating process; Step 3, subjecting the reaction system after the coating treatment to aging treatment; Step 4: After filtering, washing and drying the aged reaction system, iron red with an amphiphilic transparent surface and high oil absorption is obtained.
4. The method for preparing iron oxide red with high oil absorption having an amphiphilic transparent surface according to claim 3, characterized in that: In the step 1, the mass ratio of iron ore red powder to deionized water is 1:2-1:
6.
5. The method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface according to claim 3 or 4, characterized in that: The dispersant is sodium hexametaphosphate, sodium tripolyphosphate, sodium pyrophosphate or sodium citrate, and the mass ratio of the dispersant to deionized water is 1:400-1:
600.
6. The method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface according to claim 5, characterized in that: In the step 1, the dispersion stirring rate is 200 r / min-300 r / min, and the dispersion time is 40 min.
7. The method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface according to claim 6, characterized in that: In the step 2, the coating treatment method is: The SiO2 precursor solution is added at a uniform speed and stirred continuously for SiO2 coating. The SiO2 precursor solution is added for 60 minutes. After SiO2 coating, it is stirred for 10 minutes. Then, the Al2O3 precursor solution is added at a uniform speed and stirred continuously for Al2O3 coating. The Al2O3 precursor solution is added for 15 minutes to 75 minutes.
8. The method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface according to claim 7, characterized in that: The SiO2 precursor solution is a soluble silicate solution; the mass concentration of the SiO2 precursor solution is 10% based on SiO2; The Al2O3 precursor solution is a soluble aluminate solution; the mass concentration of the Al2O3 precursor solution is 10% based on Al2O3.
9. The method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface according to claim 8, characterized in that: In the step three, the pH value of the reaction system after the coating treatment is adjusted to 7-7.5, and the aging treatment is carried out at 50° C.-90° C. for 30 minutes.
10. The method for preparing iron oxide red with high oil absorption and having an amphiphilic transparent surface according to claim 9, characterized in that: In the step 4, after filtering the aged reaction system, deionized water is added for washing until the conductivity of the washing water is less than 200 μS / cm; the filter cake obtained by washing is dried at a temperature of 160° C.-200° C. for 3 h-5 h.