Additive for metal soft magnetic powder core and preparation method
By using additives of hydrated calcium silicate, nano-concave and concave rock stone and nanomica sheets, the lubrication and mold release problems in the preparation of metal soft magnetic powder cores are solved, the strength and insulation performance are improved, and high temperature stability and excellent magnetic properties are achieved.
Patent Information
- Application Number
- CN202411264670.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-10
AI Technical Summary
In the traditional metal soft magnetic powder core preparation process, lubricant and mold release agent evaporate during stress annealing, resulting in product appearance problems, low mechanical strength, and poor insulation performance.
Using additives composed of hydrated calcium silicate, nano-concave and concave rock stone and nanomica sheets, powder additives are prepared by adsorbing volatile lubricating oil and stirring to improve the strength and insulation of metal soft magnetic powder cores and provide them during the pressing process. Lubrication effect.
It significantly improves the strength and insulation performance of the metal soft magnetic powder core, the heat resistance temperature exceeds 800℃, no agglomeration phenomenon, the product strength increases by more than 20%, the magnetic permeability and quality factor increase by more than 2.5%, and no carbon residue affects the magnetic permeability. and dust removal system.
Smart Images

Figure BDA0005036789420000031 
Figure BDA0005036789420000041 
Figure BDA0005036789420000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of magnetic materials, and in particular relates to an additive for metal soft magnetic powder cores. Background Art
[0002] Iron silicon and iron silicon aluminum metal soft magnetic powder cores are widely used in electronic equipment due to their excellent magnetic properties and low loss. However, traditional insulation formulas and processes often fail to provide ideal insulation performance, which will increase the loss of metal soft magnetic powder cores and also have disadvantages such as low mechanical strength. The lubricants and release agents used more in the pressing process are zinc stearate and calcium stearate. These lubricants will evaporate during the subsequent stress relief annealing process, adhere to the exhaust duct when cold, and drip on the product, affecting the product appearance. When cold, they will adhere to the dust bag and block the bag. Summary of the invention
[0003] In order to solve the lubrication and demoulding problems during the pressing process of the metal soft magnetic powder core and improve the insulation and strength of the metal soft magnetic powder core, the present invention provides an additive for the metal soft magnetic powder core and a preparation method of the additive for the metal soft magnetic powder core.
[0004] An additive for a metal soft magnetic powder core is prepared by including 48-70% by weight of hydrated calcium silicate, 20-40% by weight of nano-attapulgite and 5-15% by weight of nano-mica flakes; wherein the hydrated calcium silicate adsorbs more than 2.0 mL / g of volatile lubricating oil;
[0005] The average particle size of the nano-attapulgite and nano-mica flakes is less than 1 micron;
[0006] The additive is in powder form, has a heat-resistant temperature exceeding 800° C., and has no agglomeration phenomenon.
[0007] When used for preparing a metal soft magnetic powder core, the additive is used in an amount of 0.5 to 2.5% of the mass of the metal soft magnetic powder after passivation treatment.
[0008] The preparation steps of an additive for a metal soft magnetic powder core are as follows:
[0009] (1) drying the hydrated calcium silicate, attapulgite and nano-mica flakes respectively to obtain dried hydrated calcium silicate, dried nano-attapulgite and dried nano-mica flakes;
[0010] (2) immersing the dried hydrated calcium silicate in volatile lubricating oil, stirring with a stirring paddle, and letting it stand; stirring again, and letting it stand again, with each standing time being half of each stirring time, and repeating this process 2-5 times. When the oil absorption of the hydrated calcium silicate is greater than 2.0 mL / g, removing the hydrated calcium silicate from the oil and controlling the oil to obtain oil-immersed hydrated calcium silicate;
[0011] (3) In a spiral stirrer, 48-70% by weight of oil-impregnated hydrated calcium silicate, 20-40% by weight of dried nano-attapulgite, and 5-15% by weight of dried nano-mica flakes are stirred and mixed uniformly at room temperature to obtain a powdery additive for metal soft magnetic powder cores.
[0012] The further preparation technology scheme is as follows:
[0013] In step (1), the drying temperature is 100-110° C. and the drying time is 30-40 min.
[0014] In step (1), the degree of drying is as follows: sampling is performed at intervals of 20 minutes, and the mass loss of the sample before and after drying is less than 0.3%.
[0015] In step (2), stir with a stirring paddle for 20 minutes, let stand for 10 minutes, stir for another 20 minutes, let stand for another 10 minutes, and repeat this cycle 2-5 times.
[0016] The beneficial technical effects of the present invention are embodied in the following aspects:
[0017] 1. The additive of the present invention is an inorganic additive, which utilizes the structural and performance advantages of three inorganic substances, namely, hydrated calcium silicate, nano-attapulgite and nano-mica flakes, to improve the strength, insulation and lubricity of the metal soft magnetic powder core. Hydrated calcium silicate is a new type of calcium silicate functional powder material, which has the characteristics of rich porous structure, high porosity, large specific surface area, high oil absorption rate (oil absorption is above 2.0 mL / g) and no magnetic impurities. Attapulgite is a natural, long-chain structured, hydrated magnesium-rich aluminum silicate clay mineral with strong adhesion and high temperature stability, which can improve the strength of the metal soft magnetic powder core. Nano-mica flakes are a layered silicate mineral with high mechanical strength and rigidity, good high temperature resistance and insulation properties. The above three inorganic substances are used to prepare the metal soft magnetic powder core, the strength of the metal soft magnetic powder core is mainly provided by the fibrous nano-attapulgite, the insulation is mainly provided by mica and hydrated calcium silicate, and the lubrication is mainly provided by the volatile lubricating oil adsorbed inside the hydrated calcium silicate.
[0018] 2. The heat-resistant temperature of the additive of the present invention exceeds 800°C, which significantly improves the strength of the metal soft magnetic powder core. The prepared metal soft magnetic powder core has comprehensive excellent magnetic properties and mechanical properties. The product strength is increased by at least 20%, and the magnetic permeability μ and quality factor Q value in each frequency band are increased by at least 2.5%. No die-drawing phenomenon occurs during the development process, and the lubrication performance is good.
[0019] 3. The additive of the present invention has excellent oil impregnation ability. The volatile lubricating oil is impregnated in the interior of the hydrated calcium silicate, which does not affect the fluidity of the additive itself and the metal powder. After being pressed, the interior of the hydrated calcium silicate is pressed out to play a lubricating role. In the subsequent annealing process, it can be completely volatilized below 300°C, and there will be no carbon residue (affecting the magnetic permeability) in the metal soft magnetic powder core. It will not affect the product yield and dust removal system like existing lubricants such as zinc stearate. DETAILED DESCRIPTION
[0020] The present invention will be further described below in conjunction with embodiments.
[0021] All the raw materials in the following examples are commercially available.
[0022] Example 1
[0023] The preparation steps of the additive for the metal soft magnetic powder core are as follows:
[0024] (1) First, 5 kg of hydrated calcium silicate, 4 kg of nano-attapulgite and 1 kg of nano-mica flakes were dried in an oven at a drying temperature of 110° C. for 40 min to obtain dried hydrated calcium silicate, dried nano-attapulgite and dried nano-mica flakes. Drying degree: sampling was performed at intervals of 20 min, and the mass loss of the sample before and after drying was less than 0.3%.
[0025] The average particle sizes of nano-attapulgite and nano-mica flakes are both less than 1 micron.
[0026] (2) The dried hydrated calcium silicate is put into a volatile lubricating oil, which is an aluminum foil stamping oil (AF-3R), stirred with a stirring paddle for 20 minutes, allowed to stand for 10 minutes, stirred again for 20 minutes, allowed to stand for 10 minutes, and this cycle is repeated 4 times. When the oil absorption of the hydrated calcium silicate exceeds 2.0 mL / g, the hydrated calcium silicate is removed and the oil is controlled to obtain oil-immersed hydrated calcium silicate.
[0027] (4) In a spiral stirrer, the oil-impregnated hydrated calcium silicate, the dried nano-attapulgite and the dried nano-mica flakes are stirred and mixed uniformly at room temperature to obtain a powdered additive for metal soft magnetic powder core. The heat-resistant temperature of the additive prepared in Example 1 exceeds 800° C., and there is no agglomeration phenomenon.
[0028] The additive prepared in Example 1 is mixed with FeSiAl powder that has been pre-passivated, the amount of the additive being 0.5% of the mass of the FeSiAl powder that has been pre-passivated, pressed into shape, and then subjected to stress relief annealing in a nitrogen atmosphere, and cooled to obtain a metal soft magnetic powder core.
[0029] The sendust magnetic powder core parallel samples finally obtained in Example 1 were tested three times, and the performance is shown in Table 1. At the same time, a comparative test was carried out on the same type of soft magnetic powder test powder, and the performance of comparative example 1 is also listed in Table 1.
[0030] Comparative Example 1: 0.3% of nano-silicon dioxide and 0.2% of zinc stearate were added to the mass of FeSiAl powder.
[0031] Table 1: Performance comparison between Inventive Example 1 and Comparative Example 1 (FeSiAl)
[0032]
[0033] In Table 1, μ refers to the magnetic permeability of the soft magnetic powder core, and Q refers to the quality factor of the soft magnetic powder core, and the same applies below.
[0034] Example 2
[0035] The preparation steps of the additive for the metal soft magnetic powder core are as follows:
[0036] (1) First, 8 kg of hydrated calcium silicate, 5 kg of nano-attapulgite and 2 kg of nano-mica flakes are dried in an oven at a drying temperature of 100° C. for 50 min to obtain dried hydrated calcium silicate, dried nano-attapulgite and dried nano-mica flakes. Drying degree: sampling is performed at intervals of 20 min, and the mass loss of the sample before and after drying is less than 0.3%.
[0037] The average particle sizes of nano-attapulgite and nano-mica flakes are both less than 1 micron.
[0038] (2) The dried hydrated calcium silicate is put into volatile lubricating oil, which is oil for copper tube bending, brand AF-2R, and stirred with a stirring paddle for 20 minutes, allowed to stand for 10 minutes, stirred for another 20 minutes, allowed to stand for 10 minutes, and after two cycles, when the oil absorption of the hydrated calcium silicate exceeds 2.5 mL / g, the hydrated calcium silicate is removed and the oil is controlled to obtain oil-immersed hydrated calcium silicate.
[0039] (3) In a spiral stirrer, the oil-impregnated hydrated calcium silicate, the dried nano-attapulgite and the dried nano-mica flakes are stirred and mixed at room temperature to obtain a powdered additive for metal soft magnetic powder core. The heat-resistant temperature of the additive prepared in Example 2 exceeds 800° C. without agglomeration.
[0040] The additive prepared in Example 2 is mixed with iron silicon (FeSi) powder that has been pre-passivated, and the amount of the additive is 1.5% of the mass of the iron silicon (FeSi) powder that has been pre-passivated. The powder is pressed into shape, and then stress relief annealing is performed in a nitrogen atmosphere. The powder is cooled to obtain a metal soft magnetic powder core.
[0041] Comparative Example 2 adds 1% of nano-silicon dioxide and 0.5% of zinc stearate based on the mass of iron silicon (FeSi) powder.
[0042] Table 2: Performance comparison between Inventive Example 2 and Comparative Example 2 (FeSi)
[0043]
[0044] The iron silicon magnetic powder core parallel samples finally obtained in Example 2 were tested three times, and the performance is shown in Table 2. At the same time, a comparative test was carried out on the same type of soft magnetic powder test powder, and the performance of Comparative Example 2 is also listed in Table 2.
[0045] Example 3
[0046] The preparation steps of the additive for the metal soft magnetic powder core are as follows:
[0047] (1) First, 7 kg of hydrated calcium silicate, 4 kg of nano-attapulgite and 1 kg of nano-mica flakes were dried in an oven at a drying temperature of 120° C. for 50 min to obtain dried hydrated calcium silicate, dried nano-attapulgite and dried nano-mica flakes. Drying degree: sampling was performed at intervals of 20 min, and the mass loss of the sample before and after drying was less than 0.3%.
[0048] The average particle sizes of nano-attapulgite and nano-mica flakes are both less than 1 micron.
[0049] (2) The dried hydrated calcium silicate is put into volatile lubricating oil, which is the oil for copper tube expansion head, brand K-2, and stirred with a stirring paddle for 20 minutes, allowed to stand for 10 minutes, stirred for another 20 minutes, allowed to stand for 10 minutes, and after two cycles, when the oil absorption of the hydrated calcium silicate exceeds 2.1 mL / g, the hydrated calcium silicate is removed and the oil is controlled to obtain oil-immersed hydrated calcium silicate.
[0050] (3) In a spiral stirrer, the oil-impregnated hydrated calcium silicate, the dried nano-attapulgite and the dried nano-mica flakes are stirred and mixed uniformly at room temperature to obtain a powdered additive for metal soft magnetic powder core. The heat-resistant temperature of the additive prepared in Example 3 exceeds 800° C., and there is no agglomeration phenomenon.
[0051] The additive prepared in Example 3 is mixed with iron-nickel (FeNi) powder that has been pre-passivated, and the amount of the additive accounts for 2.5% of the mass of the pre-passivated iron-nickel powder. The powder is pressed into shape, and then stress-relief annealing is performed in a nitrogen atmosphere. The powder is cooled to obtain a metal soft magnetic powder core.
[0052] Comparative Example 3 adds 1.5% of nano-silicon dioxide and 1.0% of zinc stearate based on the mass of iron-nickel (FeNi) powder.
[0053] Table 3: Performance comparison between the inventive examples and the comparative examples (FeNi)
[0054]
[0055] The iron-nickel magnetic powder core parallel samples finally obtained in this Example 3 were tested three times, and the performance is shown in Table 3. At the same time, a comparative test was carried out on the same type of soft magnetic powder test powder, and the performance of Comparative Example 3 is also listed in Table 3.
Claims
1. An additive for a metal soft magnetic powder core, characterized in that: The additive is prepared from 48-70% by weight of hydrated calcium silicate, 20-40% by weight of nano-attapulgite and 5-15% by weight of nano-mica flakes; The hydrated calcium silicate adsorbs more than 2.0 mL / g of volatile lubricating oil; The average particle size of the nano-attapulgite and nano-mica flakes is less than 1 micron; The additive is in powder form, has a heat-resistant temperature exceeding 800° C., and has no agglomeration phenomenon.
2. The additive for metal soft magnetic powder core according to claim 1, characterized in that: When used for preparing a metal soft magnetic powder core, the additive is used in an amount of 0.5 to 2.5% of the mass of the metal soft magnetic powder after passivation treatment.
3. The method for preparing an additive for a metal soft magnetic powder core according to claim 1, characterized in that: The steps are as follows: (1) The hydrated calcium silicate, attapulgite and nano-mica flakes are dried respectively to obtain dried hydrated calcium silicate, dried nano-attapulgite and dried nano-mica flakes. (2) immersing the dried hydrated calcium silicate in volatile lubricating oil, stirring with a stirring paddle, and letting it stand; stirring again, and letting it stand again, with each standing time being half of each stirring time, and repeating this process 2-5 times. When the oil absorption of the hydrated calcium silicate is greater than 2.0 mL / g, removing the hydrated calcium silicate from the oil and controlling the oil to obtain oil-absorbed hydrated calcium silicate; (3) In a spiral stirrer, 48-70% by weight of oil-absorbing hydrated calcium silicate, 20-40% by weight of dried nano-attapulgite, and 5-15% by weight of dried nano-mica flakes are stirred and mixed uniformly at room temperature to obtain a powdery additive for metal soft magnetic powder cores.
4. The preparation method according to claim 3, characterized in that: In step (1), the drying temperature is 100-110° C. and the drying time is 30-40 min.
5. The preparation method according to claim 3, characterized in that: In step (1), the degree of drying is as follows: sampling is performed at intervals of 20 minutes, and the mass loss of the sample before and after drying is less than 0.3%.
6. The preparation method according to claim 3, characterized in that: In step (2), stir with a stirring paddle for 20 minutes, let stand for 10 minutes, stir for another 20 minutes, let stand for another 10 minutes, and repeat this cycle 2-5 times.
Citation Information
Patent Citations
Electric insulated coil, rotary electric machine, and method of manufacturing for coil
CN1064171A
Copper-free ceramic friction material and preparation method thereof
EP2607335A1
Powder for sintered material
JP2010031365A
Sinterable magnetic powder composition and three-dimensional object manufactured by sintering such a composition
US20190318855A1
KR20200037174A