Ceramic coating and non-stick appliance comprising same

A ceramic coating with slow-release particles and a sealing layer addresses the short lifespan issue of ceramic coatings by maintaining non-stick properties through controlled silicone oil release, enhancing durability and performance.

CN119060568AActive Publication Date: 2024-12-03WUHAN SUPOR COOKWARE +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310649746.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Ceramic coatings for non-stick utensils have a short lifespan and fail to meet consumer demands due to rapid degradation of non-stick properties, especially under high-temperature cooking conditions and wear from metal spatulas.

Method used

A ceramic coating comprising a first layer with slow-release particles and a second sealing layer, where the slow-release particles have a porous and/or layered structure combined with silicone oil, and a second ceramic coating as a sealing layer to slow down the release of silicone oil, maintaining long-lasting non-stick properties.

Benefits of technology

The combination of slow-release particles and a sealing layer in the ceramic coating significantly enhances the non-stick performance by prolonging the release of silicone oil, ensuring continuous non-stickiness during cooking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060568A_ABST
    Figure CN119060568A_ABST
Patent Text Reader

Abstract

Provided are a ceramic coating and a non-stick appliance including the same, the ceramic coating including: a first ceramic coating including a ceramic coating precursor and sustained release particles dispersed in the ceramic coating precursor; and a second ceramic coating layer on the first ceramic coating layer and including a second ceramic coating material. The sustained-release particles comprise a sustained-release material and silicone oil combined with the sustained-release material. The slow-release material comprises at least one of vermiculite, zeolite, bentonite, diatomite, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a ceramic coating and a non-stick utensil comprising the ceramic coating. Background Art

[0002] Currently, non-stick technologies mainly include PTFE coatings and ceramic coatings. Ceramic coatings are very limited in use due to their short non-stick lifespan. They are far less widely used than PTFE products and cannot meet consumers' daily demand for non-stick utensils. For example, non-stick pans will stick to the pan after about one month of use in an average household, especially in high-temperature cooking methods such as Chinese cooking, and under the condition of wear and tear of metal spatulas, the non-stick properties decay very quickly.

[0003] Therefore, improving the long-lasting non-stick properties of ceramic coatings has become a very meaningful and urgent technical need. Summary of the invention

[0004] Based on the above-mentioned deficiencies of the prior art, the present invention provides a ceramic coating including a first ceramic coating containing slow-release particles and a second ceramic coating as a sealing layer and a non-stick utensil including the ceramic coating.

[0005] According to one aspect of an exemplary embodiment, a ceramic coating includes: a first ceramic coating formed using a first ceramic coating, the first ceramic coating including a ceramic coating precursor and slow-release particles dispersed in the ceramic coating precursor; and a second ceramic coating located on the first ceramic coating and formed using the second ceramic coating. The slow-release particles include a slow-release material and silicone oil bound to the slow-release material. The slow-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate, and layered sulfate.

[0006] The particle size of the sustained-release particles may be less than or equal to 20 microns.

[0007] The first ceramic coating may have a thickness of 10 micrometers to 80 micrometers.

[0008] The second ceramic coating may have a thickness of 8-20 microns.

[0009] The slow-release particles may be included in an amount of 5.15-32.97 parts by weight per 100 parts by weight of the first ceramic coating.

[0010] In terms of weight percentage, the silicone oil may include 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil. The molecular weight of the low molecular weight silicone oil is between 500-1000, the molecular weight of the medium molecular weight silicone oil is between 3000-6000, and the molecular weight of the high molecular weight silicone oil is between 12000-30000.

[0011] The ceramic coating precursor may include the same material as the second ceramic coating.

[0012] The first ceramic coating may include at least a first sublayer and a second sublayer stacked on each other.

[0013] The first sub-layer may be below the second sub-layer, and the content of the sustained-release particles included in the first sub-layer may be lower than the content of the sustained-release particles included in the second sub-layer.

[0014] According to another aspect of the exemplary embodiment, a non-stick utensil includes a substrate and the ceramic coating as described above disposed on the substrate.

[0015] The present invention provides a first ceramic coating by adding slow-release particles including a slow-release material to a ceramic coating. Since the slow-release material has a disordered porous and / or layered structure, in this case, silicone oil can be bound to the slow-release material. Therefore, during the cooking process, due to the porous and / or layered structure of the slow-release material, the release of silicone oil can be slowed down, thereby maintaining a long-lasting non-stick effect. In addition, the present invention provides a second ceramic coating formed by a conventional ceramic material as a sealing layer, thereby further slowing down the release of silicone oil to maintain the continuous non-stickiness of the ceramic coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a schematic diagram showing a ceramic coating according to an exemplary embodiment;

[0017] Figure 2 is an enlarged view showing slow-release particles in a ceramic coating according to an exemplary embodiment. DETAILED DESCRIPTION

[0018] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which embodiments are shown. However, the present invention may be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that the disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. The same reference numerals refer to the same elements throughout.

[0019] Ceramic coatings achieve non-stick properties mainly through the use of silicone methyl and doped silicone oil in the ceramic coating. As the product is heated and worn during use, the silicone oil in the coating will gradually be lost, destroying the silicone methyl groups on the surface, resulting in the loss of the non-stick effect, and finally the phenomenon of sticking to the pan when cooking. If the ceramic coating can store oil continuously, it can form an effective oil film to isolate the food and the coating surface, thereby achieving long-lasting non-stick properties.

[0020] Therefore, the present invention provides a ceramic coating having a first ceramic coating and a second ceramic coating, wherein the first ceramic coating includes slow-release particles containing a slow-release material, and the slow-release material may have a disordered porous and / or layered structure, and silicone oil is combined (e.g., adsorbed, bonded) to the slow-release material, so that during the cooking process, the slow-release particles slow down the release of silicone oil, thereby maintaining the long-lasting non-stick effect of the first ceramic coating. In addition, since the ceramic coating also includes a second ceramic coating as a sealing layer, the release of silicone oil in the ceramic coating can be further slowed down, thereby further enhancing the non-stick effect. However, the exemplary embodiment is not limited thereto, and those skilled in the art may apply the ceramic coating to any prior art suitable for non-stick based on the concept of the present invention.

[0021] Figure 1 is a schematic diagram showing an embodiment of a ceramic coating according to an exemplary embodiment, Figure 2 is a schematic diagram showing slow-release particles in a ceramic coating according to an exemplary embodiment. Figure 1 and Figure 2 The ceramic coating of the present invention is described.

[0022] The ceramic coating according to the present inventive concept may include a first ceramic coating and a second ceramic coating.

[0023] First Ceramic Coating

[0024] Reference Figure 1 and Figure 2 As shown, the first ceramic coating 200 according to an exemplary embodiment of the present inventive concept is formed by using a first ceramic material and is disposed on a substrate 100 . The first ceramic material includes a ceramic coating precursor 1 and slow-release particles 2 dispersed in the ceramic coating precursor.

[0025] According to an exemplary embodiment, the substrate 100 may be a substrate known in the art for making cookware, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, a titanium substrate, etc. However, the present invention does not limit the material, use, and other properties of the substrate, that is, those skilled in the art may use any material on which a ceramic coating is to be applied as the substrate 100 as needed, so that the non-stick utensil of the present invention may be applicable to any scene requiring non-stick (such as a non-stick coating of a cooking pot (e.g., a frying pan, an inner pot of an electric rice cooker), an inner and outer coating of a transport pipeline, etc.).

[0026] The first ceramic coating layer 200 is located on the substrate 100. The first ceramic coating layer 200 is formed using the first ceramic coating, and thus may include a ceramic coating precursor 1 and slow-release particles 2.

[0027] At least one of the ceramic coating precursor 1 and the second ceramic coating included in the second ceramic coating 300 to be described below may be a ceramic coating used in the art. Therefore, it may have the ingredients of the ceramic coating conventionally used in the art, so that it may be implemented using the method for preparing the ceramic coating known in the art. However, the exemplary embodiment is not limited thereto, as mentioned in the method for manufacturing the first ceramic coating using the first ceramic coating according to the present invention described below in conjunction with the exemplary embodiment, at least one of the ceramic coating precursor and the second ceramic coating may be a ceramic coating precursor prepared during the preparation of the first ceramic coating according to the present invention (and includes the same material), and the ceramic coating precursor 1 prepared by the method of the present invention to be described below may have a more excellent feature of cooperating with the slow-release particles to provide non-stickiness.

[0028] The slow-release particles 2 dispersed in the ceramic coating precursor 1 include a slow-release material 21 and silicone oil 22 bound to the slow-release material.

[0029] According to an exemplary embodiment, the slow-release material 21 may have a layer gap and / or a pore structure, so that the silicone oil 22 may be, for example, bonded to the surface of the slow-release material and / or adsorbed in the pore and / or layer gap structure. According to an example, the slow-release material 21 may include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material 21 has a porous and / or layered structure and is combined with silicone oil, so that the silicone oil 22 combined with the slow-release material 21 can be slowly released during the use of the cookware with the non-stick coating formed by the ceramic coating of the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick coating formed by the ceramic coating.

[0030] According to an exemplary embodiment, the silicone oil 22 is combined (e.g., adsorbed, bonded) to the sustained-release material 21. And provides the main non-stickiness for the ceramic coating. Here, the silicone oil 22 can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil and polyether modified silicone oil. In addition, by weight percentage, the silicone oil 22 can include 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil, wherein the molecular weight of the low molecular weight silicone oil can be between 500-1000, the molecular weight of the medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of the high molecular weight silicone oil can be between 12000-30000. Here, the silicone oil 22 can be prepared by mixing different molecular weights, because: the silicone oil with a large molecular weight is more firmly bonded to the sustained-release material and the release speed is slower; the silicone oil with a small molecular weight has better free mobility, thereby having better non-stickiness; in addition, the silicone oil with a medium molecular weight takes into account both free mobility and bonding firmness. Therefore, by combining low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil, the sustained release and non-stick effects can be better exerted.

[0031] In addition, in order to improve the bonding strength between the silicone oil and the sustained-release material, a coupling agent may be provided between the sustained-release material and the silicone oil. Here, the coupling agent may include a silane coupling agent. However, the exemplary embodiment is not limited thereto, and the coupling agent may be omitted.

[0032] Preferably, the particle size of the sustained-release particles according to the exemplary embodiment may be less than or equal to 20 micrometers. This is because an excessively large particle size (eg, greater than 20 micrometers) tends to have a large influence on the appearance of the formed non-stick coating.

[0033] According to an exemplary embodiment, in the first ceramic coating 200, 5.15-32.97 parts by weight of the slow-release particles may be included per 100 parts by weight of the first ceramic coating 200. This is because, when there is too much ceramic coating precursor, the content of the slow-release particles is relatively small, so the slow-release effect is poor; however, when the content of the slow-release particles is relatively large, the strength and bonding force of the coating are easily reduced.

[0034] Figure 1 A single-layer first ceramic coating 200 is shown applied on the substrate 100 , however, exemplary embodiments are not limited thereto, that is, the first ceramic coating may also include at least two sub-layers (eg, two layers, three layers, etc.) of ceramic coatings.

[0035] In addition, when the first ceramic coating 200 is a single layer, the single layer of the first ceramic coating 200 may have a thickness in the range of 10 micrometers to 80 micrometers. This is because when the thickness of the first ceramic coating 200 is less than 10 micrometers, the wear resistance is insufficient and the first ceramic coating is easily worn out; on the contrary, when the thickness of the first ceramic coating is greater than 80 micrometers, the coating becomes loose, thereby reducing the impact strength.

[0036] In addition, when the first ceramic coating 200 includes at least two sublayers, the at least two sublayers may be the same except for the content and particle size of the slow-release particles. For example, according to the example of including two sublayers, the first ceramic coating 200 may include a first sublayer (not shown) and a second sublayer (not shown) set from the substrate 100, and the first sublayer includes a ceramic coating precursor and first slow-release particles, the second sublayer includes a ceramic coating precursor and second slow-release particles, the content of the second slow-release particles may not be less than the content of the first slow-release particles, and the content of the second slow-release particles may be 5.15-32.97 parts by weight of the second slow-release particles per 100 parts by weight of the second sublayer, in which case the content of the first slow-release particles may be 32.97 parts by weight or less of the first slow-release particles and less than the content of the second particles per 100 parts by weight of the first sublayer. In addition, when the first ceramic coating 200 includes at least two sublayers, the thickness of the sublayer including the slow-release particles may be no less than 10 microns, and the total thickness of the at least two sublayers (ie, the thickness of the first ceramic coating 200 ) may be no greater than 80 microns.

[0037] Second ceramic coating

[0038] The second ceramic coating 300 is located on the first ceramic coating 200 .

[0039] The second ceramic coating 300 can be formed using a second ceramic coating. Here, the second ceramic coating can be the same or different from the ceramic coating precursor in the first ceramic coating (for example, it can include the same or different materials). That is, the difference between the second ceramic coating and the first ceramic coating can be only that the second ceramic coating does not include slow-release particles (or further does not include fillers), and the second ceramic coating can be a ceramic coating precursor formed during the preparation of the first ceramic coating described below or prepared using a method for preparing a ceramic coating precursor, or the second ceramic coating can be a ceramic coating commonly used in the prior art or prepared using a conventional formula. For example, according to the example, a silane substance, an alkaline silica sol and a non-stick additive can be formulated into a second ceramic coating according to a general ratio formula.

[0040] The second ceramic coating 300 does not include the slow-release particles, and serves as a sealing layer to further slow down the release of the silicone oil in the slow-release particles in the first ceramic coating 200. Therefore, the second ceramic coating 300 may have a thickness of 8 micrometers to 20 micrometers.

[0041] Above, the ceramic coating structure including the first ceramic coating 200 and the second ceramic coating 300 of the present inventive concept is described in conjunction with exemplary embodiments. Hereinafter, a method for preparing the ceramic coating including the first ceramic coating and the second ceramic coating will be described in detail.

[0042] The method for manufacturing a ceramic coating according to the present invention may include: providing a substrate 100; preparing a first ceramic coating and a second ceramic coating; forming a first ceramic coating 200 on the substrate 100 using the first ceramic coating using a layer-forming process; and forming a second ceramic coating 300 on the first ceramic coating 200 using the second ceramic coating using a layer-forming process.

[0043] According to an exemplary embodiment, the substrate 100 may be a substrate known in the art for making cookware, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, a titanium substrate, etc. However, the present invention does not limit the material, use, and other properties of the substrate, that is, those skilled in the art may use any material on which a ceramic coating is to be applied as the substrate 100 as needed.

[0044] Before, during, or after providing the substrate 100 , the first ceramic coating and the second ceramic coating may be prepared.

[0045] Preparation of the first ceramic coating and the second ceramic coating

[0046] According to an exemplary embodiment, the first ceramic coating may include a ceramic coating precursor and slow-release particles 2 dispersed in the ceramic coating precursor. Therefore, the step of preparing the first ceramic coating may include the steps of preparing the ceramic coating precursor 1 and the slow-release particles 2 separately and mixing the ceramic coating precursor 1 with the slow-release particles 2 to obtain the first ceramic coating. However, the exemplary embodiment is not limited thereto, that is, those skilled in the art may also adopt the preparation method of the ceramic coating of the prior art to obtain the ceramic coating precursor here, or may combine the step of preparing the ceramic coating precursor with the step of preparing the slow-release particles, and the redundant description of the manufacturing method of the ceramic coating of the prior art is not made here. Below, the method for preparing the first ceramic coating according to the concept of the present invention by preparing the ceramic coating precursor and the slow-release particles separately will be mainly described.

[0047] According to an exemplary embodiment, the step of preparing the ceramic coating precursor may include a step of providing materials and a step of mixing.

[0048] The step of providing materials may include the steps of separately providing A material, B material and C material.

[0049] Here, material A may include a silane substance, material B may include silica sol and filler as essential components, optional pigments, wetting agents, thickeners and emulsifiers as unnecessary components and a solvent, and material C may include an organic acid as an essential component, and optional pH buffers and catalysts (e.g., zirconium acetate) as unnecessary components.

[0050] In the A material, according to an exemplary embodiment, the silane substance is used to form polysiloxane during the formation of the ceramic coating, and therefore, the silane substance here may include a substance known in the art for polycondensation to form polysiloxane. According to an exemplary embodiment, the silane substance may include at least one of methyltrimethoxysilane, methyltriethoxysilane, and dimethyldimethoxysilane, but is not limited thereto. In addition, in addition to the silane substance, the A material may also include tetraethyl orthosilicate that is polycondensed to form polysiloxane, and in this case, in the A material, by weight percentage, the silane substance may account for 80%-97% of the A material, and the tetraethyl orthosilicate may account for 3%-20% of the A material.

[0051] Material B may necessarily include fillers and silica sol. The filler plays a role in increasing the wear resistance of the coating, etc. Therefore, the present invention does not limit the type of filler, and ordinary commonly used fillers can be selected, for example, at least one of mica powder, kaolin, montmorillonite, silicon carbide, alumina and silicon dioxide can be selected. In addition, silica sol is the main film-forming substance of ceramic coatings, which reacts with polysiloxane under acidic conditions to form a ceramic coating. Therefore, commercially available ordinary silica sol can be selected as the silica sol in material B of the present invention. For example, the silica sol can be Akzo Nobel 1050 (silica sol) or American Grace LUDIXAM-50.

[0052] The necessary components in the B material can be dispersed in a solvent. That is, the B material can also include a solvent. Here, the solvent can include deionized water, and in order to adjust the volatilization rate of the solvent during the coating drying process, the solvent can also include isopropanol. In addition, the ratio between isopropanol and water is unlimited, and the ratio between water and isopropanol can be selectively proportioned according to actual needs.

[0053] In the B material, in addition to the above-mentioned necessary components, one or more of a pigment, a wetting agent, a thickener and an emulsifier may be selectively included as an unnecessary component. Here, the pigment is mainly used to give the coating different colors, so ordinary inorganic pigments can be selected. Inorganic pigments have good temperature resistance and good safety, and inorganic pigments are preferably selected in the high temperature resistant field. According to an exemplary embodiment, at least one of carbon black, copper chrome black, titanium dioxide, iron oxide, etc. may be selected as a filler. In addition, during the preparation of the necessary components in the solvent, in order to provide the excellent properties of the material, at least one of a wetting agent, a thickener and an emulsifier may also be added to the material.

[0054] According to a specific example, the B material may include, by weight percent: 30wt%-48wt% of silica sol, 8wt%-13wt% of pigment, 8wt%-25wt% of filler, 0.2wt%-1wt% of wetting agent, 1wt%-3wt% of thickener, 3wt%-5wt% of emulsifier, and the balance is isopropyl alcohol and deionized water. However, exemplary embodiments are not limited thereto, and one or more of the unnecessary components may be omitted.

[0055] The C material is used as a strong acid catalyst, and may include an organic acid as an essential component, and an optional pH buffer and a catalyst (e.g., zirconium acetate) as an unnecessary component. Here, the organic acid is used to adjust the pH value of the silica sol in the subsequent process so that it can react with the A material in an acidic environment, and therefore, an organic acid commonly used in the art for ceramic coatings can be used. According to an exemplary embodiment, at least one of formic acid and acetic acid can be selected as an organic acid, and when both formic acid and acetic acid are included, the weight ratio between formic acid and acetic acid can be between 4:6 and 1:1. In addition, in the C material, a pH buffer and a catalyst may also be selectively included. Here, the pH buffer and the catalyst may be a pH buffer and a catalyst used in the process of preparing a strong acid catalyst for ceramic coatings known in the art, for example, the pH buffer may be a weak acid such as boric acid, and the catalyst is used to accelerate the reaction rate of the sol-gel, and may be zirconium acetate, etc. However, the exemplary embodiment is not limited to the types of pH buffers and catalysts, and suitable pH buffers and catalysts may be omitted or appropriately selected based on the prior art.

[0056] According to an exemplary embodiment, the C material may include 80-97 parts by weight of a mixture of formic acid and acetic acid, 1-2 parts by weight of a boric acid pH buffer, and 0.5 parts by weight of a zirconium acetate catalyst.

[0057] After providing the above-mentioned materials, a mixing step may be performed. Herein, the mixing step may include a first mixing step of mixing the B material with the C material and a second step of mixing the result of the first mixing step (ie, the first material described below) with the A material.

[0058] Specifically, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidic (e.g., to less than or equal to 4) by utilizing the acidity of the C material to obtain the first material. Since the C material includes a solid filler and an optional pigment, the C material can be added to a grinder and ground for 0.5h-2h before mixing or during the preparation of the C material, so that it is fully dispersed and ground to a particle size of less than or equal to 15 microns to obtain a uniformly dispersed slurry.

[0059] After the B material and the C material are mixed, the mixture may be tumbling dispersed for a predetermined time (eg, 0.5 h) so that the first material has a high degree of dispersion.

[0060] After obtaining the first material, material A may be added to the first material. Here, the weight ratio of the added amount of material A to material B may be in the range of (20-30):(40-60). After adding material A, material A and material B may be shaken evenly so that material A and material B undergo a sol-gel reaction in an acidic environment to form a ceramic coating precursor.

[0061] The slow-release particles can be prepared during, before, or after the preparation of the ceramic coating precursor. The slow-release particles can be prepared by mixing the slow-release material with silicone oil.

[0062] According to an exemplary embodiment, the sustained-release particle 2 may include a sustained-release material 21 having a pore structure and / or a layer structure and a silicone oil 22 combined with (eg, adsorbed, bonded to) the sustained-release material.

[0063] A slow-release material precursor of appropriate size (i.e., a slow-release material before grinding, when the grinding step is omitted, the slow-release material precursor can be considered as the slow-release material used in the end) can be selected to prepare slow-release particles. According to an exemplary embodiment, the slow-release material precursor can have a layer gap and / or pore structure. According to the example, the slow-release material precursor can include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material precursor has a porous and / or layered structure and the slow-release material formed after grinding is combined with silicone oil. The silicone oil combined with the slow-release material can be slowly released during the use of the cookware with a non-stick coating formed by the ceramic coating conceived by the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick layer formed by the ceramic coating.

[0064] According to an exemplary embodiment, the particle size of the slow-release material precursor may be in the range of 100 meshes to 3000 meshes (under 100 mesh sieves to on 3000 mesh sieves), and the particle size of the slow-release material within this range may obey a normal distribution. However, when the particle size is too large (e.g., on a 100 mesh sieve), the excessively large particle size is likely to increase the grinding process or make the particle size of the slow-release material after grinding too large, ultimately affecting the appearance of the non-stick coating made using the ceramic coating; on the contrary, too small a particle size (e.g., under a 3000 mesh sieve, and when the particle size is smaller after grinding) is not easy to effectively adsorb and bond silicone oil, and thus it is not easy to achieve a good silicone oil slow-release effect.

[0065] When the slow-release material precursor has the above-mentioned particle size distribution, the particle size of the slow-release material finally obtained can be made to be less than 20 microns by using two grinding processes as described below. However, the exemplary embodiment is not limited thereto, that is, when the slow-release material precursor is selected to have a smaller value within the range of 100 mesh-3000 mesh, one grinding process can be omitted; in addition, when the particle size of the slow-release material precursor is selected to have a smaller value within the above-mentioned range, two grinding processes can be omitted. When at least one of the grinding processes is omitted, the omitted grinding process can be replaced by a stirring process, or no treatment can be performed on the mixture.

[0066] According to an exemplary embodiment, the silicone oil 22 is combined (e.g., adsorbed, bonded) with the sustained-release material 21 and provides the main non-stickiness for the ceramic coating. The silicone oil can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, and polyether modified silicone oil, and can be mixed by silicone oils of different molecular weights in a certain proportion to form a silicone oil composition with a molecular weight normal distribution; wherein, by weight percentage, the low molecular weight silicone oil content can be 20wt%-30wt%, the medium molecular weight silicone oil content can be 40wt%-60wt%, and the high molecular weight silicone oil content can be 20wt%-30wt%. Here, the molecular weight of the low molecular weight silicone oil can be between 500-1000, the molecular weight of the medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of the high molecular weight silicone oil can be between 12000-30000. By utilizing a normally distributed silicone oil composition, the sustained-release and non-stick effects can be better exerted. This is because: high molecular weight silicone oil is more firmly bonded to the sustained-release material and releases more slowly; low molecular weight silicone oil has better free mobility and thus better non-stick properties; in addition, medium molecular weight silicone oil takes into account both free mobility and strong bonding. Therefore, low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil can be combined to better exert the sustained-release and non-stick effects.

[0067] According to an example, 35-58 parts by weight of a slow-release material precursor can be mixed with 42-60 parts by weight of silicone oil to obtain a mixture, and 1 part by weight of a coupling agent (e.g., a methoxysilane coupling agent), 0.3 parts by weight of a catalyst (e.g., a titanate catalyst) and 1-1.5 parts by weight of a dispersant can be added to the mixture to prepare slow-release particles. Here, the coupling agent and the catalyst are used to enhance the bonding force between the silicone oil and the slow-release material, and the dispersant is used to improve the dispersion of the slow-release material in the silicone oil. Therefore, the exemplary embodiment is not limited to the case of including a coupling agent, a dispersant and a catalyst, and at least one of the coupling agent, the catalyst and the dispersant can be omitted.

[0068] According to a specific example, the silicone oil, the sustained-release material with a particle size of 100 mesh sieve-3000 mesh sieve and the silane coupling agent can be mixed uniformly according to the above ratio, and ground to a particle size of less than or equal to 30 microns, and then the catalyst is added, and the particle size is continued to be less than or equal to 20 microns, and then ultrasonic treatment is performed at room temperature (e.g., 22°C) for 0.5h-1h, so that the sustained-release particles can be obtained. Here, firstly, the silicone oil is mixed with the sustained-release material and then ground to a particle size of less than or equal to 30 microns, so that the silicone oil and the sustained-release material can be mixed uniformly, and then, the silicone oil is ground to a particle size of less than or equal to 20 microns under the condition of the catalyst, so that the silicone oil can be fully firmly adsorbed and bonded to the outside of the sustained-release material. However, when the particle size of the sustained-release material is less than 30 microns, the first grinding can be omitted, and a stirring process can be optionally provided, or a second grinding process can be directly performed. In addition, when the particle size of the sustained-release material is less than 15 microns, the second grinding process can be further omitted, and a stirring process can be optionally provided.

[0069] After the ceramic coating precursor and the slow-release particles are prepared, the slow-release particles may be mixed with the ceramic coating precursor to prepare a ceramic coating according to an exemplary embodiment.

[0070] According to an exemplary embodiment, during the preparation of the first ceramic coating, based on the total weight of the first ceramic coating, 61-92 parts by weight of a ceramic coating precursor can be mixed with 5-30 parts by weight of slow-release particles (for example, the weight ratio of A, B, C and slow-release particles D can be (20-30): (40-60): (1-2): (5-30)), and after the ceramic coating precursor and the slow-release particles are mixed, the mixture can be stirred at a speed of 120-200 rpm for 6h-8h to obtain the desired first ceramic coating.

[0071] In addition, although the above describes a method of obtaining a ceramic coating by separately preparing a ceramic coating precursor and slow-release particles and mixing the ceramic coating precursor with the slow-release particles, in a method of combining the step of preparing a ceramic coating precursor with the step of preparing slow-release particles, as described above, after mixing the B material with the C material, the A material and the slow-release particles can be added to the mixture of the B material and the C material at the same time. For example, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidic (e.g., less than or equal to 4) by using the acidity of the C material to obtain the first material. Then, the A material and the slow-release particles can be added to the mixture, where the weight ratio of the addition amount between the A material and the B material can be in the range of (20-30): (40-60), and the addition amount of the slow-release particles can be in the range of 5.15wt%-32.97wt% based on the total weight of the mixture of A, B, C and the slow-release particles. After mixing, the mixture can be stirred at a rotation speed of 120-200 rpm for 6h-8h to obtain the desired first ceramic coating.

[0072] The method for preparing the first ceramic coating is described above. When the first ceramic coating includes a plurality of sub-layers, the method for preparing the first ceramic coating described above can be referred to to form respective corresponding sub-first ceramic coatings for different sub-layers, and each sub-first ceramic coating can differ only in the amount of slow-release particles added or the particle size of the slow-release particles. Here, those skilled in the art can easily obtain the preparation method of each sub-layer based on the preparation method of the first ceramic coating, and therefore, in order to avoid redundancy, it will not be described in detail.

[0073] The second ceramic coating may be prepared before, during or after the first ceramic coating is prepared.

[0074] According to an exemplary embodiment, the second ceramic coating may be a ceramic coating commonly used in the art, and thus, may be prepared using a conventional formula in the prior art.

[0075] According to the example, the second ceramic coating can be prepared by the following method: (1) silane and tetraethyl orthosilicate are mixed and stirred to obtain a component E silane composition; (2) silica sol is mixed with isopropyl alcohol and deionized water to obtain a component F slurry; (3) formic acid, acetic acid, a buffer (e.g., boric acid) and a catalyst (e.g., zirconium acetate) are mixed to obtain a component G strong acid catalyst; (4) the above three components are mixed in sequence according to a mass ratio of E:F:G=(20-30):(40-60):(1-2), and rolling and aging to obtain a second ceramic coating, wherein the mixing order and aging method are as follows: first, components F and G are mixed in the required number of parts, the pH is adjusted to below 4, rolling and dispersing for 0.5h, and then the required number of parts of E are added and shaken to obtain the desired ceramic coating.

[0076] After the first ceramic coating and the second ceramic coating are prepared, preparation of the first ceramic coating layer and preparation of the second ceramic coating layer may be performed.

[0077] Preparation of the first ceramic coating and the second ceramic coating

[0078] After the ceramic coating is obtained, a first ceramic coating layer 200 may be formed on the substrate 100 using a layer forming process, and a second ceramic coating layer 300 may be formed on the first ceramic coating layer 200 .

[0079] For example, the first ceramic coating and the second ceramic coating can be sprayed by air spraying. Here, the spraying of the first ceramic coating and the second ceramic coating does not limit the air spraying parameters, and the difference between the spraying of the first ceramic coating and the spraying of the second ceramic coating can only be that different thicknesses of ceramic coatings are formed by different spraying times. Here, the air spraying parameters are as follows: the spraying distance is 160mm; the air pressure is 0.3MPa; the flow rate is 8L / min. However, the exemplary embodiment is not limited to this, the parameters of the air spraying can be adaptively adjusted according to the specific process, and those skilled in the art can also use other methods of forming layers to form a ceramic coating using the first ceramic coating and the second ceramic coating conceived by the present invention. In addition, in order to improve the bonding force between the ceramic coating 200 and the substrate 100, the substrate can be treated. For example, the substrate can be sandblasted with 60# brown corundum to form a surface roughness of 3-6 microns, and then the substrate is cleaned and preheated to 40°C to 60°C, and then the ceramic coating formation process is performed.

[0080] After air spraying, the resultant may be cured at 230° C.-280° C. for 10 min-15 min to form a first ceramic coating 200 with a thickness of 10 μm-80 μm and a second ceramic coating 300 with a thickness of 8 μm-20 μm.

[0081] Through the detailed description in combination with the exemplary embodiments above, the first ceramic coating of the present invention includes slow-release particles, so that during the cooking process, the release of silicone oil can be slowed down, thereby maintaining a long-lasting non-stick effect. In addition, since the ceramic coating of the present invention further includes a second ceramic coating, the release of silicone oil can be further slowed down by the sealing effect of the second ceramic coating.

[0082] Hereinafter, the beneficial effects of the inventive concept will be described in conjunction with specific examples.

[0083] Example 1

[0084] The first ceramic coating is formed by the following method.

[0085] S1: 80 wt % of methyltrimethoxysilane and 20 wt % of ethyl orthosilicate are mixed and stirred uniformly to obtain a silane composition of component A;

[0086] S2: 30wt% of Akzo Nobel 1050 (silica sol), 8wt% of titanium dioxide (pigment), 25wt% of kaolin (filler), 3wt% of Tween-80 (emulsifier), 1wt% of water-based modified bentonite (thickener), 0.3wt% of polyoxyethylene ether TRITON X-100 (wetting agent), 20wt% of isopropanol and the balance of deionized water were mixed evenly, then added to a grinder and ground for 2h, fully dispersed and ground to a particle size of not more than 15 microns, to obtain component B slurry;

[0087] S3: 48 parts by weight of formic acid, 48 parts by weight of acetic acid, 1 part by weight of boric acid (buffer), and 0.5 parts by weight of zirconium acetate (catalyst) are uniformly mixed to obtain component C strong acid catalyst;

[0088] S4: 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 and 42 parts by weight of vermiculite (slow-release material) with a particle size of 100 to 3000 meshes are mixed, and then 3 parts by weight of methoxysilane coupling agent are added and mixed evenly, and the mixture is ground to a particle size of no more than 30 microns, and then 0.3 parts by weight of titanate (catalyst) is added, and the mixture is further ground to a particle size of no more than 20 microns, and then ultrasonically treated at room temperature of 22° C. for 0.5 h to obtain a slow-release particle component D, and the particle size of the slow-release particle component D obeys a normal distribution;

[0089] S5: The above four components are mixed in order according to the weight ratio of A: B: C: D = 20: 40: 1: 5, and rolled to mature to obtain the first ceramic coating. The mixing order and the maturation method are as follows: first, 40 parts by weight of component B and 1 part by weight of component C are mixed evenly, and the pH is adjusted to 4 by component C, and the mixture is rolled and dispersed for 0.5 hours, and then 20 parts by weight of component A are added and shaken evenly, and then 5 parts by weight of component D are added, and the reaction is stirred at a speed of 200 rpm for 8 hours to obtain the desired first ceramic coating.

[0090] The second ceramic coating was formed by the following method.

[0091] W1: 80 wt% of methyltrimethoxysilane and 20 wt% of ethyl orthosilicate are mixed and stirred uniformly to obtain a component E silane composition;

[0092] W2: 30 wt % of Akzo Nobel 1050 (silica sol), 3 wt % of Tween-80 (emulsifier), 1 wt % of water-based modified bentonite (thickener), 20 wt % of isopropanol and the remainder of deionized water were mixed uniformly to obtain component F slurry;

[0093] W3: 48 parts by weight of formic acid, 48 parts by weight of acetic acid, 1 part by weight of boric acid (buffer), and 0.5 parts by weight of zirconium acetate (catalyst) are uniformly mixed to obtain component G strong acid catalyst;

[0094] W4: The above three components are mixed in order according to the weight ratio of E: F: G = 20: 40: 1, and rolled and matured to obtain the second ceramic coating. The mixing order and the aging method are as follows: first, 40 parts by weight of component F and 1 part by weight of component G are mixed evenly, and the pH is adjusted to 4 by using component G, and the mixture is rolled and dispersed for 0.5h, and then 20 parts by weight of component E are added and shaken evenly to obtain the desired second ceramic coating.

[0095] The non-stick cookware including the first ceramic coating and the second ceramic coating is manufactured by using the first ceramic coating and the second ceramic coating by the following method.

[0096] B1: Substrate treatment. The stainless steel substrate is sandblasted with 60# brown corundum to form a surface roughness of 3 microns;

[0097] B2: Preheating. Clean the sandblasted substrate and preheat it to 60°C;

[0098] B3: Spraying. The first ceramic coating is used to form a first ceramic coating with a thickness of 80 microns on the substrate by air spraying, and the second ceramic coating is used to form a second ceramic coating with a thickness of 8 microns on the first ceramic coating. The air spraying parameters are as follows: spraying distance is 160 mm; air pressure is 0.3 MPa; flow rate is 8 L / min;

[0099] B4: Sintering: Curing at 250°C for 10 minutes.

[0100] Through the above method, the non-stick cookware of Example 1 is obtained.

[0101] Example 2

[0102] The difference from Example 1 is that the sustained-release material is bentonite.

[0103] Example 3

[0104] The difference from Example 1 is that the sustained-release material is alpha alumina.

[0105] Example 4

[0106] The difference from Example 1 is that the particle size of the sustained-release particles is less than or equal to 17 microns, and the particle size of the sustained-release particle component D obeys a normal distribution.

[0107] Example 5

[0108] The difference from Example 1 is that the particle size of the sustained-release particles is less than or equal to 12 microns, and the particle size of the sustained-release particle component D obeys a normal distribution.

[0109] Example 6

[0110] The difference from Example 1 is that the particle size of the sustained-release particles is less than or equal to 8 microns, and the particle size of the sustained-release particle component D obeys a normal distribution.

[0111] Example 7

[0112] The difference from Example 1 is that the thickness of the first ceramic coating is 10 microns.

[0113] Example 8

[0114] The difference from Example 1 is that the thickness of the first ceramic coating is 30 microns.

[0115] Example 9

[0116] The difference from Example 1 is that the thickness of the first ceramic coating is 60 microns.

[0117] Example 10

[0118] The difference from Example 1 is that the thickness of the second ceramic coating is 13 microns.

[0119] Embodiment 11

[0120] The difference from Example 1 is that the thickness of the second ceramic coating is 17 microns.

[0121] Example 12

[0122] The difference from Example 1 is that the thickness of the second ceramic coating is 20 microns.

[0123] Example 13

[0124] The difference from Example 1 is that A, B, C and D are mixed in sequence according to a weight ratio of A:B:C:D=20:40:1:12 to prepare the modified ceramic coating.

[0125] Embodiment 14

[0126] The difference from Example 1 is that A, B, C and D are mixed in sequence according to a weight ratio of A:B:C:D=20:40:1:18 to prepare the modified ceramic coating.

[0127] Embodiment 15

[0128] The difference from Example 1 is that A, B, C and D are mixed in sequence according to a weight ratio of A:B:C:D=20:40:1:29 to prepare the modified ceramic coating.

[0129] Example 16

[0130] The difference from Example 1 is that A, B, C and D are mixed in order according to the weight ratio of A:B:C:D=30:60:2:5 to prepare the modified ceramic coating.

[0131] Embodiment 17

[0132] The difference from Example 1 is:

[0133] (1) preparing a first ceramic coating 01 by using step S5;

[0134] (2) further comprising step S51, wherein the difference between step S51 and step S5 is that the components A, B, C and D obtained in steps S1 to S4 are sequentially mixed in a weight ratio of A:B:C:D=20:40:1:1 to prepare a sub-first ceramic coating 02;

[0135] (3) A first sub-layer with a thickness of 35 μm was formed on the substrate using the sub-first ceramic coating 02 by the air spraying method of Example 1, and a second sub-layer with a thickness of 45 μm was formed on the first sub-layer using the sub-first ceramic coating 01 by the air spraying method of Example 1.

[0136] Embodiment 18

[0137] The difference from Example 1 is that the silicone oil is composed of 20 wt % of hydroxy silicone oil with a molecular weight of 800, 60 wt % of hydroxy silicone oil with a molecular weight of 3000 and 20 wt % of hydroxy silicone oil with a molecular weight of 12000.

[0138] Embodiment 19

[0139] The difference from Example 1 is that the silicone oil is composed of 30 wt % of hydroxy silicone oil with a molecular weight of 800, 40 wt % of hydroxy silicone oil with a molecular weight of 3000 and 30 wt % of hydroxy silicone oil with a molecular weight of 12000.

[0140] Embodiment 20

[0141] The difference from Example 1 is that the silicone oil is composed of 25 wt % of hydroxy silicone oil with a molecular weight of 800, 50 wt % of hydroxy silicone oil with a molecular weight of 3000 and 25 wt % of hydroxy silicone oil with a molecular weight of 12000.

[0142] Embodiment 21

[0143] The difference from Example 1 is that 35 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 42 parts by weight of sustained-release material.

[0144] Embodiment 22

[0145] The difference from Example 1 is that 42 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 42 parts by weight of sustained-release material.

[0146] Embodiment 23

[0147] The difference from Example 1 is that 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 49 parts by weight of sustained-release material.

[0148] Embodiment 24

[0149] The difference from Example 1 is that 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 60 parts by weight of sustained-release material.

[0150] Comparative Example 1

[0151] The difference from Example 1 is that step S4 is omitted. That is, in step S5, components A, B and C are mixed in order according to a weight ratio of A:B:C=22:40:1, and the obtained ceramic material precursor is used to manufacture non-stick cookware.

[0152] Comparative Example 2

[0153] The difference from Example 1 is that the second ceramic coating is not included.

[0154] Comparative Example 3

[0155] The difference from Example 1 is that 30 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 60 parts by weight of sustained-release material.

[0156] Comparative Example 4

[0157] The difference from Example 1 is that 60 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 40 parts by weight of sustained-release material.

[0158] The non-stick properties of the non-stick cookware of the above-mentioned Examples 1-24 and Comparative Examples 1-4 were tested, and the test results are shown in the following table.

[0159] plan Long-lasting non-stickiness / times Example 1 13000 Example 2 11000 Example 3 12000 Example 4 12000 Example 5 11000 Example 6 8000 Example 7 9000 Example 8 12000 Example 9 13000 Example 10 14000 Embodiment 11 16000 Example 12 17000 Example 13 21000 Embodiment 14 22000 Embodiment 15 25000 Example 16 9000 Embodiment 17 13000 Embodiment 18 18000 Embodiment 19 19000 Embodiment 20 22000 Embodiment 21 12000 Embodiment 22 14000 Embodiment 23 11000 Embodiment 24 15000 Comparative Example 1 500 Comparative Example 2 11000 Comparative Example 3 8000 Comparative Example 4 9000

[0160] Performance index test

[0161] The above-obtained cookware was subjected to a performance test, and the specific performance test method is as follows:

[0162] (1) Long-lasting non-stick test method: refer to 4.2.1 Fried egg non-stick test in GB_T 32095.2-2015. The unit is the number of times. The higher the number, the longer the life. The non-stick result is evaluated once every 1000 times, and the number of times when the non-stickiness reaches Level III is recorded.

[0163] (2) Plane wear resistance test method: GB_T 32095.2-2015 4.3.1 Plane wear resistance test, use 3M7447 scouring pad, apply a force of 15N, the frequency is 33 times / minute, and the scouring pad is replaced every 500 times.

[0164] By comparing and analyzing the embodiments 1-24 of the present invention and the comparative examples 1-4, it is not difficult to find that: the long-lasting non-stickiness of the existing conventional ceramic coating in comparative example 1 does not exceed 500 times; since comparative example 2 does not include a second ceramic coating, the long-lasting non-stickiness is relatively low; the silicone oil in comparative example 3 cannot effectively provide a sustained-release effect due to its low content; in addition, the content of the sustained-release material in comparative example 4 is too low, and the amount of combined silicone oil is small, and an effective sustained-release effect cannot be formed; in comparison, the long-lasting non-stickiness of the sensible ceramic coating according to the present invention is 8000-25000 times.

[0165] Although one or more embodiments of the present invention have been described with reference to the drawings, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the claims.

Claims

1. A ceramic coating, characterized in that: The ceramic coating comprises: A first ceramic coating layer is formed using a first ceramic coating, wherein the first ceramic coating comprises a ceramic coating precursor and slow-release particles dispersed in the ceramic coating precursor; and a second ceramic coating layer, located on the first ceramic coating layer as a sealing layer and formed using a second ceramic coating, Wherein, the sustained-release particles include a sustained-release material and silicone oil bound to the sustained-release material. Wherein, the sustained-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.

2. The ceramic coating according to claim 1, characterized in that The particle size of the sustained-release particles is less than or equal to 20 microns.

3. The ceramic coating according to claim 1, characterized in that The first ceramic coating has a thickness of 10 micrometers to 80 micrometers.

4. The ceramic coating according to claim 1, characterized in that The second ceramic coating has a thickness of 8-20 microns.

5. The ceramic coating according to claim 1, characterized in that The slow-release particles are contained in an amount of 5.15-32.97 parts by weight per 100 parts by weight of the first ceramic coating.

6. The ceramic coating according to claim 1, characterized in that In terms of weight percentage, the silicone oil includes 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil. Among them, the molecular weight of low molecular weight silicone oil is between 500-1000, the molecular weight of medium molecular weight silicone oil is between 3000-6000, and the molecular weight of high molecular weight silicone oil is between 12000-30000.

7. The ceramic coating according to claim 1, characterized in that The ceramic coating precursor and the second ceramic coating include the same material.

8. The ceramic coating according to claim 1, characterized in that The first ceramic coating includes at least a first sublayer and a second sublayer stacked on each other.

9. The ceramic coating according to claim 1, characterized in that The first sub-layer is below the second sub-layer, and the content of the sustained-release particles included in the first sub-layer is lower than the content of the sustained-release particles included in the second sub-layer.

10. A non-stick utensil, characterized in that: The non-stick utensil comprises a substrate and a ceramic coating as claimed in any one of claims 1 to 9 disposed on the substrate.

Citation Information

Patent Citations

  • Titanium-containing ceramic paint and protective coating

    CN103013193A

  • Non-stick ceramic coating for cooking utensils and preparation method thereof

    CN112759963A

  • Modified ceramic coating, composite coating, preparation methods of modified ceramic coating and composite coating, and cooker

    CN115820116A

  • Long-term high-temperature-resistant non-stick ceramic coating as well as preparation method and application thereof

    CN115926498A

  • Modified ceramic coating, composite coating, preparation methods of modified ceramic coating and composite coating, and cooker