Environment-friendly carbon nanotube antistatic agent, coating, composite material and assembly

By optimizing the preparation of efficient and environmentally friendly carbon nanotube antistatic agents, combined with aqueous resins and carbon nanotubes, the existing antistatic agents are solved for the inconvenience of environmental and use, achieving efficient and environmentally friendly electrostatic protection effects, and reducing costs and improve stability.

CN119060577AInactive Publication Date: 2024-12-03ZHEJIANG NAKO NANO NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411575575.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing antistatic agents are prone to volatile organic matter during the preparation process, which is harmful to the preparation personnel and the environment. Solvents need to be added during use, which is inconvenient to use.

Method used

Using optimized preparation of environmentally friendly carbon nanotube antistatic agents, including multi-walled carbon nanotubes in high defect states and single-walled carbon nanotubes in low defect states, combined with aqueous resin, it is formulated through specific heat treatment and infrared Raman spectroscopy to form high efficiency. The antistatic coating reduces the dosage of additives and improves coating performance and conductivity.

Benefits of technology

It achieves environmentally friendly and efficient anti-static effect without additional solvents, reduces application costs, improves the stability of the slurry system and the high-temperature and anti-aging performance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an environment-friendly carbon nano tube antistatic agent, a coating, a composite material and an assembly, the antistatic agent comprises the following components in parts by weight: 0.5-2 parts of multi-walled carbon nano tube, and the multi-walled carbon nano tube is in a high defect state; 0.1 to 0.2 part of a single-walled carbon nanotube, wherein the single-walled carbon nanotube is in a low defect state; 4-8 parts of water-based resin; and 100 parts of water. According to the invention, by optimizing the composition of the product and through a coating system with better dispersibility, the coating performance and conductivity of the product are improved, and the use amount of auxiliaries is reduced, so that the application cost is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to electronic material technology, in particular to an environmentally friendly carbon nanotube antistatic agent, coating, composite material and component. Background Art

[0002] Films will accumulate static electricity during die-cutting or use. When a large amount of static electricity accumulates, it will cause damage to warehouses or equipment and easily cause fires. When the electronics industry uses protective films and other films, when a large amount of static electricity accumulates and the voltage is too high, it is easy to break down electronic equipment, causing the electronic equipment to be paralyzed and damaged. Static electricity will absorb dust and impurities in the air, so it is necessary to remove static electricity on the surface of objects in a clean environment. Spraying or directly applying a layer of antistatic agent on the surface of the object can avoid the impact of static electricity and eliminate or reduce the harm caused by static electricity.

[0003] Most of the antistatic agents used for antistatic film surfaces on the market are oily antistatic agents. Such antistatic agents are prone to produce volatile organic matter during the preparation process, which is harmful to the preparation personnel and the environment. Other solvents need to be added for coating and spraying during use, which is inconvenient to use.

[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0005] The purpose of the present invention is to provide an environmentally friendly carbon nanotube antistatic agent and film, which improves the coating performance and electrical conductivity of the product by optimizing the composition of the product, reduces the amount of additives used, thereby effectively reducing the application cost and improving the stability of the slurry system itself.

[0006] To achieve the above-mentioned purpose, an embodiment of the present invention provides an environmentally friendly carbon nanotube antistatic agent, which comprises, by weight: 0.5-2 parts of multi-walled carbon nanotubes, which are highly defective; 0.1-0.2 parts of single-walled carbon nanotubes, which are low-defective; 4-8 parts of water-based resin; and 100 parts of water.

[0007] In one or more embodiments of the present invention, the specific surface area of ​​the single-walled carbon nanotubes and multi-walled carbon nanotubes is 100-300 m 2 / g (BET SSA).

[0008] In one or more embodiments of the present invention, the diameters of the single-walled carbon nanotubes and the multi-walled carbon nanotubes are both 2-13 nm and the lengths are 1.5-10 μm.

[0009] In one or more embodiments of the present invention, the high defect state is expressed as measured by the peak intensity of infrared Raman spectroscopy: I (1780 cm -1 ) / I(1580cm -1 )=1.2-1.3.

[0010] Preferably, the high defect state is achieved by rapidly heating the nanotube from room temperature to 800° C. to 1100° C. at a heating rate of 30 to 50° C. / min under the protection of an inert gas and then annealing the nanotube for 2 h to 4 h.

[0011] In one or more embodiments of the present invention, the low defect state is expressed as measured by the peak intensity of infrared Raman spectroscopy: I (1319 cm -1 ) / I(1580cm -1 )=0.5-0.8.

[0012] Preferably, the low defect state is achieved by heating the nanotubes from room temperature to 600° C. to 800° C. at a heating rate of 10 to 30° C. / min under the protection of an inert gas and then annealing for 1 to 2 hours.

[0013] In one or more embodiments of the present invention, the mass ratio of multi-walled carbon nanotubes to single-walled carbon nanotubes is (7-8):1.

[0014] In one or more embodiments of the present invention, the aqueous resin is selected from polyethylene glycol having a number average molecular weight of 60,000 to 100,000.

[0015] In one or more embodiments of the present invention, the coating is a layer structure of at least one layer or multiple layers formed by the antistatic agent as described above, such as an antistatic coating of an antistatic film on the surface of a liquid crystal display.

[0016] The composite material comprises a carrier and the above-mentioned coating formed on the surface of the carrier.

[0017] The component comprises a light-transmitting functional body and a shell formed around the functional body for at least electrostatic isolation, wherein the shell is at least partially formed of the composite material as described above.

[0018] In one or more embodiments of the present invention, the coating slurry can be prepared by rapidly dispersing a dispersant, an aqueous resin, an antistatic agent, and deionized water in a high-speed mixer at a speed of 400-600 rpm for 3-5 minutes.

[0019] In one or more embodiments of the present invention, the composite material includes a main body and the aforementioned coating formed on the surface of the main body, such as an antistatic film on the surface of a liquid crystal display.

[0020] Compared with the prior art, the environmentally friendly carbon nanotube antistatic agent and film according to the embodiment of the present invention use the modified carbon nanotubes to provide conductive properties as an optimized antistatic agent, and then add resin and water, and mix them according to a certain ratio, reducing the amount and type of auxiliary agents, thereby effectively reducing the application cost, improving the stability of the slurry system itself, and obtaining an antistatic agent with environmentally friendly carbon nanotubes as the system. The environmentally friendly carbon nanotube antistatic agent of the present invention can be applied to the surface of PET, PVC and plastic products by roller coating, spraying, printing and other purposes, without the need for additional solvent dilution, and can have a good antistatic effect. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is described in detail below in conjunction with the specific embodiments of the present invention. However, it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0022] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0023] Example 1: The environmentally friendly carbon nanotube antistatic agent of this example comprises, by weight: 0.5 parts of a specific surface area of ​​100 m 2 / g (BET SSA) of multi-walled carbon nanotubes (2nm in diameter, 1.5μm in length), which are highly defective; 0.1 part specific surface area is 100 m 2 / g (BET SSA) of single-walled carbon nanotubes (diameter 2nm, length 1.5μm), the single-walled carbon nanotubes are in a low-defect state; 4 parts of polyethylene glycol with a number average molecular weight of 60,000; 100 parts of water.

[0024] The high defect state is achieved by rapidly heating the nanotube from room temperature to 800°C at a rate of 30°C / min under the protection of an inert gas and then annealing for 2 hours. The peak intensity of the sample measured by infrared Raman spectroscopy is about: I (1780cm -1 ) / I(1580cm -1 )=1.21.

[0025] The low defect state is achieved by heating the nanotubes from room temperature to 600°C at a rate of 10°C / min under the protection of an inert gas and then annealing for 1 hour. The peak intensity of the sample measured by infrared Raman spectroscopy is about: I (1319 cm -1 ) / I(1580cm -1 )=0.50.

[0026] Before coating, the antistatic agent can be the aforementioned aqueous resin, carbon nanotubes, and deionized water, which are quickly dispersed into a slurry in a high-speed mixer at a speed of 500 rpm for 4 minutes, so that a protective film can be obtained after coating. These protective films can be used in occasions such as displays that require electrostatic protection.

[0027] Embodiment 2: The difference between this embodiment and embodiment 1 is only that: The high defect state is achieved by rapidly heating the nanotube from room temperature to 1000°C at a rate of 40°C / min under the protection of an inert gas and then annealing for 3 h. The peak intensity of the sample is measured by the infrared Raman spectrum: I (1780 cm -1 ) / I(1580cm -1 )=1.26.

[0028] The low defect state is achieved by heating the nanotubes from room temperature to 700°C at a rate of 20°C / min under the protection of an inert gas and then annealing for 1.5 h. The peak intensity of the sample is measured by the infrared Raman spectrum: I (1319 cm -1 ) / I(1580cm -1 )=0.68.

[0029] Embodiment 3: This embodiment differs from Embodiment 1 only in that: The high defect state is achieved by rapidly heating the nanotube from room temperature to 1100°C at a rate of 50°C / min under the protection of inert gas and then annealing for 4 h. The peak intensity of the sample is measured by infrared Raman spectroscopy: I (1780 cm -1 ) / I(1580cm -1 )=1.29.

[0030] The low defect state is achieved by heating the nanotubes from room temperature to 800°C at a rate of 30°C / min under the protection of an inert gas and then annealing for 2 h. The peak intensity of the sample is measured by the infrared Raman spectrum: I (1319 cm -1 ) / I(1580cm -1 )=0.78.

[0031] Embodiment 4: This embodiment differs from Embodiment 2 only in that: 1 specific surface area is 200m 2 / g (BET SSA) of multi-walled carbon nanotubes (diameter 7nm, length 5μm), multi-walled carbon nanotubes are highly defective; 0.15 parts of the specific surface area is 200m 2 / g (BET SSA) of single-walled carbon nanotubes (diameter 6nm, length 6μm), the single-walled carbon nanotubes are in a low-defect state; 6 parts of polyethylene glycol with a number average molecular weight of 80,000; 100 parts of water.

[0032] Embodiment 5: This embodiment differs from Embodiment 2 only in that: 2 parts with a specific surface area of ​​300m 2 / g (BET SSA) of multi-walled carbon nanotubes (diameter 13nm, length 10μm), multi-walled carbon nanotubes are highly defective; 0.2 parts of the specific surface area is 300m 2 / g (BET SSA) of single-walled carbon nanotubes (diameter 13nm, length 10μm), the single-walled carbon nanotubes are low-defect state; 8 parts of polyethylene glycol with a number average molecular weight of 100,000; 100 parts of water.

[0033] Embodiment 6: This embodiment differs from Embodiment 2 only in that: 0.8 parts of multi-walled carbon nanotubes; 0.1 parts of single-walled carbon nanotubes.

[0034] Embodiment 7: The difference between this embodiment and embodiment 2 is only that: 1.4 parts of multi-walled carbon nanotubes; 0.2 parts of single-walled carbon nanotubes.

[0035] Embodiment 8: The difference between this embodiment and embodiment 7 is only that: 1.05 parts of multi-walled carbon nanotubes; 0.15 parts of single-walled carbon nanotubes.

[0036] Embodiment 9: The difference between this embodiment and embodiment 2 is that: The water-based resin is polypropylene alcohol with the same molecular weight.

[0037] Comparative Example 1: The difference between this comparative example and Example 2 is that the multi-walled carbon nanotubes are in a non-defective state, that is, they are not subjected to the heating and heat preservation annealing treatment.

[0038] Comparative Example 2: The difference between this comparative example and Example 2 is that the single-walled carbon nanotubes are in a non-defective state, that is, they are not subjected to the heating and heat preservation annealing treatment.

[0039] Comparative Example 3: The difference between this comparative example and Example 2 is that the multi-walled carbon nanotubes are in a low defect state: that is, the temperature is raised from room temperature to 700°C at a rate of 20°C / min under the protection of an inert gas and then annealed for 1.5h. The peak intensity of the sample is measured by the infrared Raman spectrum: I (1319cm -1 ) / I(1580cm -1 )=0.52. Single-walled carbon nanotubes are highly defective: that is, the nanotubes are rapidly heated from room temperature to 1000°C at a rate of 40°C / min under the protection of inert gas and then annealed for 3 hours. The peak intensity of the sample is measured by infrared Raman spectroscopy: I (1780cm -1 ) / I(1580cm -1 )=1.35.

[0040] Comparative Example 4: The difference between this comparative example and Example 2 is that the dispersant W193-113 is additionally added.

[0041] Table 1

[0042]

[0043] The good stability in Table 1 above does not only refer to good dispersion uniformity of each component in the coating, but also has good thermal shock stability (tested with ±20℃ thermal shock cycle for 20 times, the antistatic coating has no obvious deformation, warping, peeling and other defects) and high temperature and anti-aging stability (tested at 50℃ and 85% humidity for 3000h, the antistatic coating has no obvious deformation, embrittlement, peeling and other defects); similarly, better indicates that the dispersion uniformity is general, the film layer has defects in the coating state, and the thermal shock stability and high temperature and anti-aging stability are manifested as defects in the local film layer; weak is worse, indicating that there are significant defects in dispersion, film forming, thermal shock stability and high temperature and anti-aging stability.

[0044] Including but not limited to the antistatic agent of the above embodiment, when coating, the coating slurry can be a dispersant, an aqueous resin, an antistatic auxiliary agent, and deionized water, which are quickly dispersed in a high-speed mixer at a speed of 400-600 rpm for 3-5 minutes. The specific mixing process can be determined according to the needs. No specific limitation is made here, and only some feasible examples are given.

[0045] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. An environmentally friendly carbon nanotube antistatic agent, comprising, by weight: 0.5 to 2 parts of multi-walled carbon nanotubes, wherein the multi-walled carbon nanotubes are highly defective, and the highly defective state is expressed as measured by the peak intensity of infrared Raman spectroscopy: I (1780 cm -1 ) / I(1580cm -1 )=1.2-1.3; 0.1-0.2 parts of single-walled carbon nanotubes, wherein the single-walled carbon nanotubes are low-defective, and the low-defective state is expressed as measured by the peak intensity of infrared Raman spectroscopy: I (1319 cm -1 ) / I(1580cm -1 )=0.5-0.8; 4~8 parts of water-based resin; 100 parts water.

2. The environmentally friendly carbon nanotube antistatic agent according to claim 1, characterized in that: The specific surface area of ​​the single-walled carbon nanotubes and multi-walled carbon nanotubes is 100-300 m 2 / g.

3. The environmentally friendly carbon nanotube antistatic agent according to claim 2, characterized in that: The single-walled carbon nanotubes and multi-walled carbon nanotubes have diameters of 2-13 nm and lengths of 1.5-10 μm.

4. The environmentally friendly carbon nanotube antistatic agent according to any one of claims 1 to 3, characterized in that: The mass ratio of the multi-walled carbon nanotubes to the single-walled carbon nanotubes is (7-8):

1.

5. The environmentally friendly carbon nanotube antistatic agent according to claim 1, characterized in that: The water-based resin is selected from polyethylene glycol with a number average molecular weight of 60,000 to 100,000.

6. A coating, a layer structure of one or more layers formed by at least the antistatic agent according to any one of claims 1 to 5.

7. A composite material comprising a carrier and the coating according to claim 6 formed on the surface of the carrier.

8. A component comprising a light-transmitting functional body and a shell formed around the functional body for at least electrostatic isolation, wherein the shell is at least partially formed of the composite material according to claim 7.

Citation Information

Patent Citations

  • Preparation method and application of defective carbon nanotubes

    CN109174074A

  • Environment-friendly carbon nanotube antistatic agent and film

    CN114958062A

  • Antistatic coating for fingerprint sensor, preparation method of antistatic coating and fingerprint sensor

    CN117247691A

  • Antistatic coating composition, antistatic sheet and sheet employing the same, method of manufacturing the same and antistatic product employing the same

    KR1020100133075A

  • Carbon nanotube dispersion liquid composition and method for manufacturing of the same, conductive coating liquid composition comprising the same, antistatic film and display device using the same

    US20160152843A1

Cited By

  • Preparation method of ultraviolet curing antistatic coating with phase separation characteristic

    CN119505588A