Easy-to-clean highlight varnish coating composition for surface coating of carbon fiber composite material as well as preparation method and application of easy-to-clean highlight varnish coating composition
By using easy-to-clean high-gloss varnish coating composition on the surface of carbon fiber composite materials, the problem of difficult cleaning of high-gloss varnish pollution in the prior art is solved, and low-temperature curing, easy-to-clean, recoating and high transparency are achieved. The effect meets the application needs of carbon fiber composite materials.
Patent Information
- Application Number
- CN202411300635.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-18
AI Technical Summary
Existing carbon fiber composite high-gloss varnishes are easily contaminated after use outdoors and are difficult to clean. The varnish with graffiti resistance has insufficient recoating properties and cannot meet the application needs of carbon fiber composites.
A easy-to-clean high-gloss varnish coating composition is adopted, which comprises component A and component B. Component A is composed of hydroxyacrylic resin, silicone modified acrylic resin, ultraviolet light absorber and light stabilizer. Component B is cured by isocyanate. The agent and solvent are composed of low-temperature curing and specific additive formulations to form a paint film with low-temperature curing, easy to clean, recoating and high transparency.
It realizes the high transparency and beautiful high-gloss varnish effect of carbon fiber composite surface, has good weather resistance and easy cleaning performance, can remove pollution through simple wipe, and is suitable for automotive exterior parts and other applications.
Smart Images

Figure BDA0005047551080000051 
Figure BDA0005047551080000061 
Figure BDA0005047551080000062
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of surface coating of carbon fiber composite materials, and specifically comprises an easy-to-clean high-gloss varnish coating composition for surface coating of carbon fiber composite materials, and a preparation method and application thereof. Background Art
[0002] As a new type of material with low density, high strength and high stiffness, carbon fiber composite material (CFRP) is becoming one of the most popular lightweight materials in the fields of automobiles, rail transportation vehicles, sports equipment, etc. When it is used for the exterior surface of transportation vehicles such as rail transportation and automobiles, in order to improve the appearance and protect the substrate, the carbon fiber composite material generally needs to be coated. In order to present the special texture weaving effect of carbon fiber, most of the existing technologies use high-gloss varnish transparent coating to coat the carbon fiber composite material. However, the current high-gloss varnish is easily contaminated by dust, oil, hand sweat, etc. in the environment under outdoor use. After contamination, it is difficult to remove it by simple methods such as wiping, and it generally requires the help of high-pressure steam shock to clean it. Therefore, after long-term outdoor use, it is difficult for the surface of the high-gloss varnish to maintain high appearance requirements. In addition, the varnish with anti-graffiti performance commonly used on the market generally requires high-temperature curing, and it is difficult to balance the anti-graffiti effect and recoatability of the paint film when using graffiti additives. For carbon fiber composite materials with high recoatability requirements, the application is seriously hindered.
[0003] In view of this, how to design an easy-to-clean high-gloss varnish coating composition that can be used for surface coating of carbon fiber composite materials, so as to achieve the high-gloss varnish effect of giving the carbon fiber composite materials a visible fiber texture while having excellent low-temperature curing, easy cleaning, recoatability, high transparency, beautiful appearance and chemical resistance and other characteristics, thereby eliminating the above-mentioned defects and deficiencies in the prior art and better serving the use needs of exterior coatings such as vehicles, is a topic that needs to be urgently solved by relevant technical personnel in the industry. Summary of the invention
[0004] In view of the above problems existing in the prior art, the first object of the present invention is to provide an easy-to-clean high-gloss varnish coating composition for surface coating of carbon fiber composite materials.
[0005] The second object of the present invention is to provide a method for preparing the clear coating composition as described above.
[0006] The third object of the present invention is to provide a surface treatment method.
[0007] To achieve the above first object, the technical solution adopted by the present invention includes:
[0008] The present invention discloses an easy-to-clean high-gloss varnish coating composition for surface coating of carbon fiber composite materials, wherein the varnish coating composition comprises component A and component B;
[0009] The component A comprises the following raw material components in parts by weight:
[0010] 20-80 parts of hydroxy acrylic resin, 3-30 parts of silicone modified acrylic resin, 10-35 parts of a first solvent, 0.5-3 parts of an ultraviolet light absorber, 0.5-2 parts of a light stabilizer, and 0.1-3 parts of an additional auxiliary agent;
[0011] The component B comprises the following raw material components in parts by weight:
[0012] 40-90 parts of isocyanate curing agent and 10-60 parts of a second solvent;
[0013] Wherein, the weight ratio of component A to component B is 1:10-10:1;
[0014] The organosilicon-modified acrylic resin is a modified resin obtained by reacting a polyacrylate resin containing a hydroxyl functional group with an organosilicon oligomer containing a hydroxyl or alkoxy functional group.
[0015] Further, the component A comprises the following raw material components in parts by weight:
[0016] 30-50 parts of hydroxy acrylic resin, 5-20 parts of organosilicon modified acrylic resin, 10-35 parts of a first solvent, 0.5-3 parts of an ultraviolet light absorber, 0.5-2 parts of a light stabilizer, and 0.1-3 parts of an external auxiliary agent.
[0017] Furthermore, the weight ratio of component A to component B is 1:5-5:1.
[0018] Furthermore, the organosilicon-modified acrylic resin is selected from modified acrylic resins with a water contact angle greater than 100°.
[0019] Furthermore, the silicone-modified acrylic resin includes but is not limited to the commercially available JZ-9522 and / or JZ-9540;
[0020] The hydroxyl value of the hydroxy acrylic resin is between 0.5% and 8%.
[0021] Furthermore, the hydroxylated acrylic resin includes but is not limited to one or more of Setalux 1907BA-75, TIRES 2850, SETALUX 1774SS-65, SETALUX 1215BA-68, SETALUX 1274BA-70 from Allnex, Joncryl 507, Joncryl 804, Joncryl 910 from BASF, and Hypomer MT-2550K, Hypomer MT-2550F, and Hypomer MT-2350 from Elementis.
[0022] Furthermore, the isocyanate curing agent includes, but is not limited to, one or more of aliphatic isocyanate polymers, alicyclic isocyanate polymers, aromatic isocyanate polymers, isocyanate hybrids, and isocyanate hybrid polymers.
[0023] Further, the first solvent and the second solvent are independently selected from one or more of hexane, heptane, toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isophorone, butyl acetate, ethyl acetate, 3-ethoxypropionic acid ethyl ester, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene carbonate, dimethyl carbonate, No. 100 solvent oil, No. 150 solvent oil, and No. 200 solvent oil.
[0024] Furthermore, the additional additives include one or more of a drying agent, a substrate wetting agent, a wetting and dispersing agent, a leveling agent, and a rheological additive.
[0025] Furthermore, the viscosity of the varnish coating composition at 23° C. is in the range of 100-10000 mPa·s, preferably 100-5000 mPa·s.
[0026] To achieve the above second purpose, the technical solution adopted by the present invention includes:
[0027] The present invention discloses a method for preparing the above-mentioned varnish coating composition, comprising the following steps:
[0028] (1) adding a hydroxy acrylic resin, a silicone-modified acrylic resin, an additional additive, an ultraviolet light absorber, a light stabilizer and a first solvent into a first container under stirring, and stirring until the mixture is uniformly mixed to obtain the component A;
[0029] (2) adding an isocyanate curing agent and a second solvent into a second container under stirring, and stirring until the mixture is uniform, thereby obtaining the component B;
[0030] (3) Component A and component B are mixed according to a certain proportion to obtain the clear coating composition.
[0031] To achieve the third objective, the technical solution adopted by the present invention includes:
[0032] The present invention discloses a surface treatment method, which comprises coating at least one layer of the clear coating composition as described above on at least one surface of a carbon fiber composite material.
[0033] Furthermore, the coating method is selected from air spraying, airless spraying, online electrostatic spraying or in-mold coating.
[0034] Beneficial effects of the present invention:
[0035] Compared with the prior art, the technical solution provided by the present invention has the following advantages:
[0036] The easy-to-clean high-gloss varnish coating composition of the present invention can impart high transparency and beautiful high-gloss varnish effect to the carbon fiber composite material, and the carbon fiber texture of the composite material is clearly visible.
[0037] The easy-to-clean high-gloss varnish coating composition of the present invention has good weather resistance, and can play a good protective role on the surface of the carbon fiber composite material after adding an ultraviolet light absorber and a light stabilizer.
[0038] The easy-to-clean high-gloss varnish coating composition of the present invention has the characteristics of low-temperature curing, easy cleaning, recoatability, high transparency, beautiful appearance and chemical resistance, and can meet the application requirements of carbon fiber composite material automotive exterior parts. DETAILED DESCRIPTION
[0039] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be clear that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] In the case of illustrating and explaining the purpose of the present invention through the following examples, the components of the composition are explained in parts by weight as a general standard. Unless otherwise specified, for the sake of simplicity, the "parts" described in the examples of the present invention have the same meaning as parts by weight.
[0041] It should be noted that the easy-to-clean performance of the varnish coating composition in the present invention refers to the fact that when the paint film is contaminated by dust, oil, sweat, etc., if it is easy to remove by simple means such as wiping, it is considered to have easy-to-clean performance. This is different from the traditional anti-graffiti performance, which means that it is not easy to leave traces of contamination on the paint film. Therefore, even if an anti-graffiti additive is added to the formula, the effect of easy removal of stains may not be obvious, and it is easy to cause re-coating problems, which greatly affects the application of coatings in carbon fiber composite materials.
[0042] In order to obtain a two-component varnish coating composition that is easy to clean, has high gloss, has a low curing temperature and good recoatability, the present invention introduces a specific type of silicone-modified acrylic resin into the varnish coating composition formula, which can impart good easy-to-clean performance to the paint film after addition, and can further improve the comprehensive performance of the paint film after curing with a hydroxyl acrylic resin and an isocyanate curing agent, and will not cause recoating problems when applied to the surface of a carbon fiber composite material.
[0043] Specifically, the present invention provides an easy-to-clean high-gloss varnish coating composition for surface coating of carbon fiber composite materials, wherein the varnish coating composition comprises component A and component B;
[0044] The component A comprises the following raw material components in parts by weight:
[0045] 20-80 parts of hydroxy acrylic resin, 3-30 parts of silicone modified acrylic resin, 10-35 parts of a first solvent, 0.5-3 parts of an ultraviolet light absorber, 0.5-2 parts of a light stabilizer, and 0.1-3 parts of an additional auxiliary agent;
[0046] The component B comprises the following raw material components in parts by weight:
[0047] 40-90 parts of isocyanate curing agent and 10-60 parts of a second solvent;
[0048] Wherein, the weight ratio of component A to component B is 1:10-10:1;
[0049] The organosilicon-modified acrylic resin is a modified resin obtained by reacting a polyacrylate resin containing a hydroxyl functional group with an organosilicon oligomer containing a hydroxyl or alkoxy functional group.
[0050] The varnish coating composition provided by the present invention has a good decorative and protective effect on the surface of the carbon fiber composite material, has high transparency and glossiness, and makes the carbon fiber composite material have a clearly visible fiber texture. At the same time, the varnish coating composition has the characteristics of low temperature curing, easy cleaning, good recoating and chemical resistance, and the carbon fiber composite material coated with the varnish can meet the application requirements of automobile exterior parts.
[0051] Further, the formula of component A is optimized, specifically including the following raw material components in parts by weight:
[0052] 30-50 parts of hydroxy acrylic resin, 5-20 parts of organosilicon modified acrylic resin, 10-35 parts of a first solvent, 0.5-3 parts of an ultraviolet light absorber, 0.5-2 parts of a light stabilizer, and 0.1-3 parts of an external auxiliary agent.
[0053] Further, the weight ratio of component A to component B is 1:5-5:1; illustratively, the weight ratio of component A to component B can be 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, etc.
[0054] Furthermore, the organosilicon-modified acrylic resin used in the present invention is a commercially available product, which has large hydrophobicity (water contact angle>100°), oleophobicity, and excellent solvent wiping resistance. The formed paint film can remove pollutants adhering to the surface of the paint film by simple methods such as wiping, and no longer needs to be cleaned by traditional high-pressure steam shock methods, which reduces the adverse effects of high-pressure steam shock on the paint film, makes the cleaning method more convenient, and also ensures the recoatability of the coating, which is difficult to achieve for many self-cleaning coatings at present. Exemplarily, the organosilicon-modified acrylic resin includes but is not limited to the commercially available ones of Jiazhixinnuo Company. JZ-9522 and / or JZ-9540.
[0055] Further, the hydroxy acrylic resin is polymerized from acrylic acid monomers, methacrylic acid monomers and their derivatives, and is selected from commercially available hydroxy acrylic resins with a hydroxy value of 0.5-8%. It has abundant active hydroxyl groups that can be cross-linked with other components of the varnish coating composition to improve the adhesion of the paint film to the carbon fiber composite material. At the same time, the hydroxy acrylic resin has good compatibility with additives and is easy to disperse. Exemplarily, the hydroxy acrylic resin includes but is not limited to Setalux1907BA-75, TIRES2850, SETALUX 1774SS-65, SETALUX 1215BA-68, SETALUX1274BA-70 of Allnex, Joncryl 507, Joncryl 804, Joncryl 910 of BASF, and one or more of Hypomer MT-2550K, Hypomer MT-2550F, and Hypomer MT-2350 of Elementis.
[0056] Further, the isocyanate curing agent includes but is not limited to one or more of aliphatic isocyanate polymers, alicyclic isocyanate polymers, aromatic isocyanate polymers, isocyanate hybrids, and isocyanate hybrid polymers. More specifically, the isocyanate curing agent can be any commercially available isocyanate curing agent that meets the above description, including but not limited to Desmodur N 3300, Desmodur N 3390, Desmodur N3600, Desmodur N 3900, and Desmodur Z 4470 sold by Bayer MaterialScience, or HDT-90, HDT-100, and HDT-LV sold by Rhodia Group, or Basonat HI100 sold by BASF.
[0057] Further, the first solvent and the second solvent may be the same or different, including but not limited to hexane, heptane, toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isophorone, butyl acetate, ethyl acetate, 3-ethoxypropionic acid ethyl ester, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene carbonate, dimethyl carbonate, No. 100 solvent oil, No. 150 solvent oil, No. 200 solvent oil, etc.
[0058] Furthermore, the ultraviolet light absorber includes but is not limited to one or more of Tinuvin 328, Tinuvin 384-2, Tinuvin 900, Tinuvin 928, Tinuvin 1130, Tinuvin 400, Tinuvin 479, Tinuvin 477, and Tinuvin CarboProtect.
[0059] Furthermore, the light stabilizer includes but is not limited to one or more of Tinuvin 144, Tinuvin 123, Tinuvin 292, Tinuvin 440 and Tinuvin 622.
[0060] Furthermore, the additional additives include one or more of a drying agent, a substrate wetting agent, a wetting and dispersing agent, a leveling agent, and a rheological additive. It should be understood by those skilled in the art that the additives can be selected according to actual process requirements, and the scope of other additives that can be used in the present invention is not limited to the additives listed above.
[0061] Furthermore, component A may contain 0.01-0.5 parts of a drying agent; component A may contain 0.01-0.5 parts of a substrate wetting agent; component A may contain 0.01-0.5 parts of a wetting and dispersing agent; component A may contain 0.01-1 parts of a leveling agent; and component A may contain 0.1-1.0 parts of a rheological additive.
[0062] Furthermore, the viscosity of the varnish coating composition at 23° C. is in the range of 100-10000 mPa·s, preferably 100-5000 mPa·s.
[0063] The present invention also provides a method for preparing the varnish coating composition as described above, comprising the steps of:
[0064] (1) Preparation of component A
[0065] Under stirring, 20-80 parts of hydroxy acrylic resin, 3-30 parts of silicone modified acrylic resin, 0.1-3 parts of external additives, 0.5-3 parts of ultraviolet light absorber and 0.5-2 parts of light stabilizer are added to the first container, and 10-35 parts of the first solvent are provided for dispersion, and stirred until the mixture is uniformly mixed to obtain the component A;
[0066] (2) Preparation of component B
[0067] Under stirring, adding 40-90 parts of isocyanate curing agent into the second container, and providing 10-60 parts of a second solvent for dispersion, wherein the second solvent is pre-filled with an inert gas to eliminate the influence of oxygen, and stirring until the mixture is uniformly mixed to obtain the component B;
[0068] (3) Component A and component B are fully mixed in a weight ratio of 1:10 to 10:1 to obtain the varnish coating composition.
[0069] The present invention also provides a surface treatment method, which comprises coating at least one layer of the varnish coating composition of the present invention as described above on at least one surface of the carbon fiber composite material, especially on an epoxy-based carbon fiber composite material substrate, curing at 60-90°C for 40-80 minutes, and repeating the above coating and curing operations 1-4 times to obtain an easy-to-clean high-gloss varnish coating.
[0070] Furthermore, the coating formed by the single coating has a thickness of 40-60 μm; and the dry film thickness of the easy-to-clean high-gloss varnish coating is 100-200 μm.
[0071] Furthermore, the coating method is selected from air spraying, airless spraying, online electrostatic spraying or in-mold coating.
[0072] The following will provide further details through specific embodiments.
[0073] Example 1
[0074] In this embodiment, a clear varnish coating composition 1 with high gloss and easy to clean is provided. The clear varnish coating composition 1 with high gloss and easy to clean comprises component A and component B. The compositions of component A and component B are as follows in parts by weight:
[0075] Table 1.1 Composition of component A in Example 1
[0076]
[0077] Table 1.2 Composition of component B in Example 1
[0078]
[0079]
[0080] The specific steps of the preparation method and application of the above-mentioned easy-to-clean high-gloss varnish coating composition 1 are as follows:
[0081] (1) Add SETALUX 1774SS-65, JZ-9540, butyl acetate and propylene glycol methyl ether acetate are stirred for 15-20 minutes at a stirring rate of 500-1500 rpm to make them evenly mixed, and then Tego wet 270, BYK-315N, Tinuvin 1130 and Tinuvin 292 are added and stirred for 20-30 minutes to obtain component A. The viscosity of component A at 23°C is in the range of 500-1000 mPa·s.
[0082] (2) Nitrogen is charged into a composite solvent of butyl acetate and propylene glycol methyl ether acetate, and Desmodur N 3390 is added under stirring. The mixture is stirred for 10-20 minutes to obtain component B, wherein the mass percentage of the isocyanate curing agent in component B is 70%.
[0083] (3) When in use, component A and component B are fully mixed at a weight ratio of 3:1 to obtain the easy-to-clean high-gloss varnish coating composition 1.
[0084] The easy-to-clean high-gloss varnish coating composition 1 is applied to an epoxy-based carbon fiber composite material substrate coated with a transparent primer, and cured at 80°C for 60 minutes to obtain a varnish coating having a dry film thickness of 40-50 μm. Performance tests are then performed, and the relevant results are shown in Table 6.
[0085] Example 2
[0086] In this embodiment, an easy-to-clean high-gloss varnish coating composition 2 is provided, and the easy-to-clean high-gloss varnish coating composition 2 includes component A and component B. In parts by weight, the compositions of component A and component B are as follows:
[0087] Table 2.1 Composition of component A in Example 2
[0088]
[0089] Table 2.2 Composition of component B in Example 2
[0090] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0091] The specific steps of the preparation method and application of the easy-to-clean high-gloss varnish coating composition 2 are as follows:
[0092] (1) Add SETALUX 1774SS-65, JZ-9540, butyl acetate and propylene glycol methyl ether acetate are stirred for 15-20 minutes at a stirring rate of 500-1500 rpm to make them evenly mixed, and then Tego wet 270, BYK-315N, Tinuvin 1130 and Tinuvin 292 are added and stirred for 20-30 minutes to obtain component A. The viscosity of component A at 23°C is in the range of 500-1000 mPa·s.
[0093] (2) Nitrogen is charged into the composite solvent of butyl acetate and propylene glycol methyl ether acetate, and Desmodur N 3390 is added under stirring, and stirred for 10-20 minutes to obtain component B. The mass percentage of the isocyanate curing agent in component B is 70%.
[0094] (3) When in use, component A and component B are fully mixed at a weight ratio of 3:1 to obtain the easy-to-clean high-gloss varnish coating composition 2.
[0095] The easy-to-clean high-gloss varnish coating composition 2 is applied to an epoxy-based carbon fiber composite material substrate coated with a transparent primer, and cured at 80°C for 60 minutes to obtain an easy-to-clean high-gloss varnish coating, the dry film thickness of the easy-to-clean high-gloss varnish coating is 40-50 μm, and then a performance test is carried out. The relevant results are shown in Table 6.
[0096] Comparative Example 1
[0097] In this comparative example, a varnish coating composition 1 is provided, and the varnish coating composition 1 comprises component A and component B. In parts by weight, the compositions of component A and component B are as follows:
[0098] Table 3.1 Composition of component A in comparative example 1
[0099]
[0100] Table 3.2 Composition of component B in comparative example 1
[0101] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0102] The specific steps of the preparation method of the above-mentioned varnish coating composition 1 are as follows:
[0103] (1) Add SETALUX 1774SS-65, JZ-9540, butyl acetate and propylene glycol methyl ether acetate are stirred for 15-20 minutes at a stirring rate of 500-1500 rpm to make them evenly mixed, and then Tego wet 270, BYK-315N, Tinuvin 1130 and Tinuvin 292 are added and stirred for 20-30 minutes to obtain component A. The viscosity of component A at 23°C is in the range of 500-1000 mPa·s.
[0104] (2) Nitrogen is charged into a composite solvent of butyl acetate and propylene glycol methyl ether acetate, and Desmodur N 3390 is added under stirring. The mixture is stirred for 10-20 minutes to obtain component B, wherein the mass percentage of the isocyanate curing agent in component B is 70%.
[0105] (3) When in use, component A and component B are fully mixed at a weight ratio of 3:1 to obtain the varnish coating composition 1.
[0106] The varnish coating composition 1 was applied to the epoxy-based carbon fiber composite material substrate coated with a transparent primer, and cured at 80°C for 60 minutes to obtain a varnish coating having a dry film thickness of 40-50 μm. The performance test was then carried out, and the relevant results are shown in Table 6.
[0107] Example 3
[0108] In this embodiment, an easy-to-clean high-gloss varnish coating composition 3 is provided. The easy-to-clean high-gloss varnish coating composition 3 includes component A and component B. In parts by weight, the compositions of component A and component B are as follows:
[0109] Table 4.1 Composition of component A in Example 3
[0110]
[0111] Table 4.2 Composition of component B in Example 3
[0112] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0113] The specific steps of the preparation method of the easy-to-clean high-gloss varnish coating composition 3 are as follows:
[0114] (1) Add SETALUX 1774SS-65, JZ-9522, butyl acetate and propylene glycol methyl ether acetate are stirred for 15-20 minutes at a stirring rate of 500-1500 rpm to make them uniformly mixed, and then Tego wet 270, BYK-315N, Tinuvin 1130 and Tinuvin 292 are added and stirred for 20-30 minutes to obtain component A. The viscosity of component A at 23°C is 500-1000 mPa·s.
[0115] (2) Nitrogen is charged into a composite solvent of butyl acetate and propylene glycol methyl ether acetate, and Desmodur N 3390 is added under stirring, and stirred for 10-20 minutes to obtain component B. The mass percentage of the isocyanate curing agent in component B is 70%.
[0116] (3) When in use, component A and component B are fully mixed at a weight ratio of 3:1 to obtain the easy-to-clean high-gloss varnish coating composition 3.
[0117] The easy-to-clean high-gloss varnish coating composition 3 is applied to the epoxy-based carbon fiber composite material substrate coated with a transparent primer, and cured at 80°C for 60 minutes to obtain a varnish coating with a dry film thickness of 40-50 μm. The performance test is then carried out, and the relevant results are shown in Table 6.
[0118] Comparative Example 2
[0119] In this comparative example, a varnish coating composition 2 is provided, wherein the varnish coating composition 2 comprises component A and component B, wherein, by weight, the compositions of component A and component B are as follows:
[0120] Table 5.1 Composition of component A in comparative example 2
[0121]
[0122] Table 5.2 Composition of component B in comparative example 2
[0123] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0124] It should be noted that: in this example, component A contains only hydroxy acrylic resin and no silicone-modified acrylic resin. Its easy-to-clean effect is mainly achieved by adding an anti-graffiti additive. Protect 5000N is implemented, so it is not within the scope of the present invention and is therefore used as Comparative Example 2.
[0125] The specific steps of the preparation method of the varnish coating composition 2 are as follows:
[0126] (1) Add SETALUX 1774SS-65, butyl acetate and propylene glycol methyl ether acetate to the main container in sequence under stirring, and stir for 15-20 minutes at a stirring rate of 500-1500 rpm. After mixing evenly, add Protect 5000N, stir for 15-20 minutes, and control the stirring rate at 500-1500 rpm. After mixing evenly, add Tego wet 270, BYK-315N, Tinuvin 1130, and Tinuvin 292, and continue stirring for 20-30 minutes to obtain component A. The viscosity of component A at 23°C ranges from 500 to 1000 mPa·s.
[0127] (2) Nitrogen is charged into the composite solvent of butyl acetate and propylene glycol methyl ether acetate, and Desmodur N 3390 is added under stirring, and stirred for 10-20 minutes to obtain component B. The mass percentage of the isocyanate curing agent in component B is 70%.
[0128] (3) When in use, component A and component B are fully mixed at a weight ratio of 3:1 to obtain the varnish coating composition 2.
[0129] The varnish coating composition 2 was applied to the epoxy carbon fiber composite material substrate coated with a transparent primer, and cured at 80°C for 60 minutes to obtain a varnish coating having a dry film thickness of 40-50 μm. The performance test was then carried out, and the relevant results are shown in Table 6.
[0130] Comparative Example 3
[0131] In this comparative example, a varnish coating composition 3 is provided, which is a commercially available nano self-cleaning varnish product (NOVclean produced by Guangzhou Sysmec). TM Self-cleaning nano coating), the product is a single component.
[0132] The varnish coating composition 3 was applied to the epoxy-based carbon fiber composite material substrate coated with a transparent primer, and cured at 80°C for 60 minutes to obtain a varnish coating having a dry film thickness of 5-10 μm. The performance test was then carried out, and the relevant results are shown in Table 6.
[0133] Comparison results
[0134] In this embodiment, the easy-to-clean high-gloss varnish coating composition 1 of Example 1, the easy-to-clean high-gloss varnish coating composition 2 of Example 2, the easy-to-clean high-gloss varnish coating composition 3 of Example 3, the varnish coating composition 1 of Comparative Example 1, the varnish coating composition 2 of Comparative Example 2, and the varnish coating composition 3 of Comparative Example 3 are compared.
[0135] The performance test results of each sample are shown in Table 6.
[0136] Table 6 Performance test results of each coating composition on carbon fiber composite material samples
[0137]
[0138] The easy-to-clean effect is achieved by writing on the coating surface with an oil-based marker pen and then directly wiping it with a non-woven fabric. Here, the applicant uses a carbon fiber composite material sample as a substrate to prepare the above coatings (Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3) with the same film thickness to compare the easy-to-clean effects of the above coatings.
[0139] The results of Table 6 show that in terms of gloss, pencil hardness, substrate adhesion, gasoline resistance and light aging resistance, the performance of Examples 1-3 is basically equivalent to that of Comparative Examples 1-2, but since Comparative Example 3 cannot be completely cured at 80°C*60min, the hardness, gloss and substrate adhesion of the formed coating are all poor, and the gasoline resistance and light aging resistance cannot be tested. In terms of easy-to-clean effect, Examples 1-3 and Comparative Example 2 are significantly better than Comparative Example 3, also because Comparative Example 3 has poor film formation under this curing condition. However, in terms of recoating adhesion, it is found that Comparative Examples 1-3 are all poor. Among them, Examples 1-2 and Comparative Example 1 show that as the amount of organosilicon-modified acrylic resin increases, the easy-to-clean effect gradually increases, but when the amount of organosilicon-modified acrylic resin reaches a certain value, the recoating adhesion cannot meet the requirements. Therefore, the amount of organosilicon-modified acrylic resin needs to be reasonably controlled to meet the balance between easy-to-clean effect and recoating adhesion. Secondly, Comparative Example 2 shows that the anti-graffiti additive has a significant effect on the recoating property of the paint film, which is not applicable to the requirements of carbon fiber multi-coating.
[0140] The present invention is described in this specification only in more preferred specific embodiments, the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the present invention. Any technical solutions that can be obtained by those skilled in the art through logical analysis, reasoning or limited experiments according to the concept of the present invention should be within the protection scope of the present invention.
Claims
1. An easy-to-clean high-gloss varnish coating composition for surface coating of carbon fiber composite materials, characterized in that: The clearcoat coating composition comprises component A and component B; The component A comprises the following raw material components in parts by weight: 20-80 parts of hydroxy acrylic resin, 3-30 parts of silicone modified acrylic resin, 10-35 parts of a first solvent, 0.5-3 parts of an ultraviolet light absorber, 0.5-2 parts of a light stabilizer, and 0.1-3 parts of an additional auxiliary agent; The component B comprises the following raw material components in parts by weight: 40-90 parts of isocyanate curing agent and 10-60 parts of a second solvent; Wherein, the weight ratio of component A to component B is 1:10-10:1; The organosilicon-modified acrylic resin is a modified resin obtained by reacting a polyacrylate resin containing a hydroxyl functional group with an organosilicon oligomer containing a hydroxyl or alkoxy functional group.
2. The clear coating composition according to claim 1, characterized in that The component A comprises the following raw material components in parts by weight: 30-50 parts of hydroxy acrylic resin, 5-20 parts of organosilicon modified acrylic resin, 10-35 parts of a first solvent, 0.5-3 parts of an ultraviolet light absorber, 0.5-2 parts of a light stabilizer, and 0.1-3 parts of an additional auxiliary agent; Preferably, the weight ratio of component A to component B is 1:5-5:
1.
3. The clear coating composition according to claim 1, characterized in that The organosilicon-modified acrylic resin is selected from modified acrylic resins with a water contact angle of >100°; Preferably, the silicone-modified acrylic resin is selected from the commercially available JZ-9522 and / or JZ-9540; The hydroxyl value of the hydroxy acrylic resin is between 0.5-8%; Preferably, the hydroxy acrylic resin is selected from one or more of Setalux 1907BA-75, TIRES2850, SETALUX 1774SS-65, SETALUX 1215BA-68, SETALUX 1274BA-70 of Allnex, Joncryl507, Joncryl 804, Joncryl 910 of BASF, Hypomer MT-2550K, Hypomer MT-2550F, Hypomer MT-2350 of Elementis.
4. The clear coating composition according to claim 1, characterized in that The isocyanate curing agent is selected from one or more of aliphatic isocyanate polymers, alicyclic isocyanate polymers, aromatic isocyanate polymers, isocyanate hybrids, and isocyanate hybrid polymers.
5. The clear coating composition according to claim 1, characterized in that: The first solvent and the second solvent are independently selected from one or more of hexane, heptane, toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isophorone, butyl acetate, ethyl acetate, ethyl 3-ethoxypropionate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene carbonate, dimethyl carbonate, No. 100 solvent oil, No. 150 solvent oil, and No. 200 solvent oil.
6. The clear coating composition according to claim 1, characterized in that The additional additives include one or more of a drying agent, a substrate wetting agent, a wetting and dispersing agent, a leveling agent, and a rheological additive.
7. The clear coating composition according to claim 1, characterized in that The viscosity of the varnish coating composition at 23° C. is in the range of 100-10000 mPa·s, preferably 100-5000 mPa·s.
8. The method for preparing the varnish coating composition according to any one of claims 1 to 7, characterized in that: The following steps are included: (1) adding a hydroxy acrylic resin, a silicone-modified acrylic resin, an additional additive, an ultraviolet light absorber, a light stabilizer and a first solvent into a first container under stirring, and stirring until the mixture is uniformly mixed to obtain the component A; (2) adding an isocyanate curing agent and a second solvent into a second container under stirring, and stirring until the mixture is uniform, thereby obtaining the component B; (3) Component A and component B are mixed in proportion to obtain the varnish coating composition.
9. A surface treatment method, characterized in that: The surface treatment method comprises coating at least one layer of the varnish coating composition according to any one of claims 1 to 7 on at least one surface of the carbon fiber composite material.
10. The surface treatment method according to claim 9, characterized in that: The coating method is selected from air spraying, airless spraying, online electrostatic spraying or in-mold coating.
Citation Information
Patent Citations
Acrylic topcoat used for vehicle frame and preparation method of acrylic topcoat
CN109971330A
Anti-bird droppings varnish and preparation method thereof
CN117487413A
Anti-contamination finish paint composition as well as preparation method and application thereof
CN118421181A
Silicone resin coated sheet
JP1998100328A
Composition of two component type dual curing clear coat for car
KR1020110060584A
Cited By
Highlight varnish with ultraviolet aging resistance and wear resistance as well as preparation method and application of highlight varnish
CN119735981A