Water-based transparent paint and preparation method thereof
By using a combination of hydroxyacrylic resin and water-based epoxy modified acrylic resin in water-based transparent paint, combining resins with different viscosity and modified transparent powder, the problem of insufficient water resistance and mechanical properties of water-based transparent paint is solved, and the water-based transparent paint is significantly improved. Performance in humid environments.
Patent Information
- Application Number
- CN202411364114.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-28
- Publication Date
- 2024-12-03
AI Technical Summary
At present, the water-based transparent paint has poor water resistance and insufficient mechanical properties, which leads to bubbles or falling off during long-term contact with water or humid environments, reducing its service life.
Using a combination of hydroxyacrylic resins and aqueous epoxy modified acrylic resins, the dispersant is enhanced by adjusting its weight ratio and using hydroxyacrylic resins of different viscosity, and using acrylonitrile-styrene-acrylate copolymer to modify transparent powders. Combination with anti-deposition agent improves the density and stability of the paint film.
It significantly improves the water resistance and mechanical properties of water-based transparent paint, making it better in terms of external forces and moisture penetration, and extends its service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to a water-based transparent paint and a preparation method thereof. Background Art
[0002] Water-based transparent paint is a transparent paint with water as a diluent. This paint uses water as a solvent, which greatly reduces the use of organic solvents and reduces the pollution to the atmosphere. It is a green and environmentally friendly transparent paint. In addition, water-based transparent paint has the advantages of good adhesion, safety, non-flammability, and high transparency. It can be used for the surface treatment of wooden products such as furniture and wooden floors. It can not only protect the wood from the external environment, but also highlight the natural texture and color of the wood, and increase the aesthetics. In addition, water-based transparent paint can also be used for the surface coating of metal products. While increasing the gloss and aesthetics of the metal, it can also prevent the metal from rusting and corrosion. The application field is very wide. Although water-based transparent paint has many advantages, it still has defects. The current water-based transparent paint uses water as a solvent, and its water resistance is relatively poor. When exposed to water or in a humid environment for a long time, the transparent paint may have problems such as bubbles or shedding. While the water resistance is reduced, its mechanical properties will also decrease, thereby reducing its service life. Therefore, improving the water resistance and mechanical properties of water-based transparent paint is a technical problem that needs to be solved urgently. Summary of the invention
[0003] The invention provides a water-based transparent paint and a preparation method thereof, which solves the problems of poor water resistance and poor mechanical properties of the water-based transparent paint in the related art.
[0004] The technical solution of the present invention is as follows: The present invention provides a water-based transparent paint, comprising the following components in parts by weight: 30-50 parts of acrylic resin, 20-30 parts of transparent powder, 1-3 parts of dispersant, 1-2 parts of anti-settling agent, 0.5-1.5 parts of curing agent, 50 parts of water; The acrylic resin includes hydroxy acrylic resin and waterborne epoxy modified acrylic resin, and the weight ratio of the hydroxy acrylic resin to the waterborne epoxy modified acrylic resin is 1:9-9:1.
[0005] As a further technical solution, the weight ratio of the hydroxyl acrylic resin to the waterborne epoxy modified acrylic resin is 3~7:1.
[0006] When the weight ratio of hydroxy acrylic resin to waterborne epoxy modified acrylic resin is 3 to 7:1, the water resistance and mechanical properties of the waterborne clear paint can be further improved.
[0007] As a further technical solution, the hydroxylated acrylic resin includes a first hydroxylated acrylic resin and a second hydroxylated acrylic resin, and the first hydroxylated acrylic resin and the second hydroxylated acrylic resin have different viscosities.
[0008] As a further technical solution, the viscosity of the first hydroxy acrylic resin is 2800-4500 mPa·s, and the viscosity of the second hydroxy acrylic resin is 1400-2500 mPa·s.
[0009] When the hydroxy acrylic resin includes a first hydroxy acrylic resin and a second hydroxy acrylic resin, the inventors found that the water resistance and mechanical properties of the water-based clear paint can be further improved by using two hydroxy acrylic resins with different viscosities in combination. It is speculated that the synergy of the two hydroxy acrylic resins with different viscosities can make the water-based clear paint more uniform and dense, thereby further improving the water resistance and mechanical properties of the water-based clear paint.
[0010] As a further technical solution, the weight ratio of the first hydroxyl acrylic resin to the second hydroxyl acrylic resin is 3-4:2.
[0011] When the weight ratio of the first hydroxy acrylic resin to the second hydroxy acrylic resin is 3 to 4:2, the water resistance and mechanical properties of the water-based clear paint can be further improved.
[0012] As a further technical solution, the transparent powder is a modified transparent powder, and the raw materials of the modified transparent powder include transparent powder and acrylonitrile-styrene-acrylate copolymer.
[0013] Modifying the transparent powder with acrylonitrile-styrene-acrylate copolymer can not only make the transparent powder disperse more evenly, but also strengthen the interface bonding with acrylic resin, thereby further improving the water resistance and mechanical properties of water-based transparent paint.
[0014] As a further technical solution, the weight ratio of the transparent powder to the acrylonitrile-styrene-acrylate copolymer is 7-23:1.
[0015] When the weight ratio of the transparent powder to the acrylonitrile-styrene-acrylate copolymer is 7 to 23:1, the water resistance and mechanical properties of the water-based transparent paint can be further improved.
[0016] As a further technical solution, the preparation method of the modified transparent powder includes the following steps: dissolving the acrylonitrile-styrene-acrylate copolymer in dimethylformamide to obtain an acrylonitrile-styrene-acrylate copolymer solution, adding the transparent powder to the acrylonitrile-styrene-acrylate copolymer solution, dispersing evenly, concentrating, and drying to obtain the modified transparent powder.
[0017] As a further technical solution, the mass fraction of the acrylonitrile-styrene-acrylate copolymer solution is 5% to 10%.
[0018] As a further technical solution, the dispersant includes one or more of sodium oleate, polyvinyl alcohol, and sodium stearate; the anti-settling agent includes one or two of organic bentonite and fumed silica; and the curing agent includes one or two of aqueous isocyanate and triethylenetetramine.
[0019] The present invention also provides a method for preparing a water-based transparent paint, comprising the following steps: mixing and stirring the components in parts by weight to obtain the water-based transparent paint.
[0020] As a further technical solution, during the mixing, the temperature is 80-90° C., during the stirring, the stirring speed is 200-300 r / min, and the stirring time is 40-60 min.
[0021] The working principle and beneficial effects of the present invention are: In the present invention, the components of the water-based clear paint include two acrylic resins, namely, hydroxy acrylic resin and water-based epoxy modified acrylic resin. The combined use of hydroxy acrylic resin and water-based epoxy modified acrylic resin can produce a synergistic effect, which can not only balance the flexibility and hardness of the water-based clear paint, so that it can better resist damage when subjected to external forces and improve its mechanical properties, but also form a more compact and stable coating structure, effectively blocking water penetration, thereby improving the water resistance of the water-based clear paint. When the weight ratio of the hydroxy acrylic resin to the water-based epoxy modified acrylic resin is 1:9 to 9:1, this synergistic effect is more excellent, and the water resistance and mechanical properties of the water-based clear paint can be significantly improved. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In the following examples and comparative examples, the model of waterborne epoxy modified acrylic resin is TY-102A; the model of acrylonitrile-styrene-acrylate copolymer is LI-931; the particle size of transparent powder is 1250 mesh; the model of organic bentonite is BP-202B; and the model of polyvinyl alcohol is PVA424H.
[0024] Example 1 A water-based transparent paint comprises the following components in parts by weight: 30 parts of acrylic resin, 20 parts of transparent powder, 1 part of polyvinyl alcohol, 1 part of organic bentonite, 0.5 parts of triethylenetetramine, 50 parts of water; The acrylic resin includes 3 parts of hydroxy acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) and 27 parts of waterborne epoxy modified acrylic resin; The preparation method of water-based transparent paint comprises the following steps: mixing components in parts by weight at 85° C. and stirring at a stirring speed of 200 r / min for 60 minutes to obtain water-based transparent paint.
[0025] Example 2 A water-based transparent paint comprises the following components in parts by weight: 40 parts of acrylic resin, 24 parts of transparent powder, 2 parts of polyvinyl alcohol, 1.5 parts of organic bentonite, 1 part of triethylenetetramine, 50 parts of water; The acrylic resin includes 20 parts of hydroxy acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) and 20 parts of waterborne epoxy modified acrylic resin; The preparation method of water-based transparent paint comprises the following steps: mixing components in parts by weight at 85° C. and stirring at a stirring speed of 250 r / min for 50 minutes to obtain water-based transparent paint.
[0026] Example 3 A water-based transparent paint comprises the following components in parts by weight: 50 parts of acrylic resin, 30 parts of transparent powder, 3 parts of polyvinyl alcohol, 2 parts of organic bentonite, 1.5 parts of triethylenetetramine, 50 parts of water; The acrylic resin includes 45 parts of hydroxy acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) and 5 parts of waterborne epoxy modified acrylic resin; The preparation method of water-based transparent paint comprises the following steps: mixing components in parts by weight at 85° C. and stirring at a stirring speed of 300 r / min for 40 minutes to obtain water-based transparent paint.
[0027] Example 4 The difference between this embodiment and embodiment 2 is that, in this embodiment, 36 parts of hydroxyl acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are added, and 4 parts of waterborne epoxy modified acrylic resin are added.
[0028] Example 5 The difference between this embodiment and embodiment 2 is that, in this embodiment, 35 parts of hydroxyl acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are added, and 5 parts of waterborne epoxy modified acrylic resin are added.
[0029] Example 6 The difference between this embodiment and embodiment 2 is that, in this embodiment, 30 parts of hydroxyl acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are added, and 10 parts of waterborne epoxy modified acrylic resin are added.
[0030] Example 7 The only difference between this embodiment and embodiment 6 is that in this embodiment, 30 parts of hydroxyl acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are replaced by an equal amount of hydroxyl acrylic resin (viscosity of 1400-2500 mPa·s, model 829-80A).
[0031] Example 8 The only difference between this embodiment and embodiment 6 is that in this embodiment, 30 parts of hydroxyl acrylic resin (viscosity of 2800~4500mPa·s, model FS-2050) are replaced by 16 parts of hydroxyl acrylic resin (viscosity of 2800~4500mPa·s, model FS-2050) and 14 parts of hydroxyl acrylic resin (viscosity of 1400~2500mPa·s, model 829-80A).
[0032] Example 9 The only difference between this embodiment and embodiment 8 is that in this embodiment, 22 parts of hydroxyl acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are added, and 8 parts of hydroxyl acrylic resin (viscosity of 1400-2500 mPa·s, model 829-80A) are added.
[0033] Example 10 The only difference between this embodiment and embodiment 8 is that in this embodiment, 18 parts of hydroxyl acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are added, and 12 parts of hydroxyl acrylic resin (viscosity of 1400-2500 mPa·s, model 829-80A) are added.
[0034] Embodiment 11 The only difference between this embodiment and embodiment 8 is that in this embodiment, 20 parts of hydroxyl acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are added, and 10 parts of hydroxyl acrylic resin (viscosity of 1400-2500 mPa·s, model 829-80A) are added.
[0035] Example 12 The only difference between this embodiment and embodiment 11 is that in this embodiment, the transparent powder is a modified transparent powder, and its preparation method comprises the following steps: dissolving 4 parts of acrylonitrile-styrene-acrylate copolymer in dimethylformamide to obtain a 5% by mass acrylonitrile-styrene-acrylate copolymer solution, adding 20 parts of transparent powder to the 5% by mass acrylonitrile-styrene-acrylate copolymer solution, dispersing evenly, concentrating, and drying to obtain a modified transparent powder.
[0036] Embodiment 13 The only difference between this embodiment and embodiment 12 is that, in this embodiment, 23.5 parts of transparent powder and 0.5 parts of acrylonitrile-styrene-acrylate copolymer are added.
[0037] Embodiment 14 The only difference between this embodiment and embodiment 12 is that, in this embodiment, 21 parts of transparent powder and 3 parts of acrylonitrile-styrene-acrylate copolymer are added.
[0038] Embodiment 15 The only difference between this embodiment and embodiment 12 is that, in this embodiment, 23 parts of transparent powder and 1 part of acrylonitrile-styrene-acrylate copolymer are added.
[0039] Comparative Example 1 The difference between this comparative example and Example 1 is that in this comparative example, no waterborne epoxy modified acrylic resin is added, and 30 parts of hydroxy acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) are added.
[0040] Comparative Example 2 The difference between this comparative example and Example 1 is that in this comparative example, no hydroxy acrylic resin (viscosity of 2800-4500 mPa·s, model FS-2050) is added, and 30 parts of waterborne epoxy-modified acrylic resin are added.
[0041] Experimental Example 1 Water resistance test The water-based transparent paints prepared in Examples 1 to 15 and Comparative Examples 1 to 2 were used to prepare and maintain coating samples with a size of 150 mm × 150 mm and a thickness of 1.5 mm according to the method in GB / T 16777-2008 "Test Methods for Building Waterproof Coatings". The samples were immersed in water at 40° C., and the time when bubbling of the samples began to appear was observed and recorded.
[0042] Experimental Example 2 Mechanical Properties Test The water-based transparent paints prepared in Examples 1 to 15 and Comparative Examples 1 to 2 were tested for tensile strength according to the method in GB / T 16777-2008 “Test methods for building waterproof coatings”, wherein the tensile speed was 200 mm / min.
[0043] The test results are shown in Table 1 below: Table 1 Test results
[0044] Compared with Comparative Examples 1-2, the tensile strength of the water-based clear paint prepared in Example 1 is significantly improved, and the time for bubbling to begin to appear when immersed in water at 40°C is significantly increased, indicating that when the components of the water-based clear paint include two acrylic resins, hydroxyl acrylic resin and water-based epoxy-modified acrylic resin, the two acrylic resins have a synergistic effect and can significantly improve the water resistance and mechanical properties of the water-based clear paint.
[0045] Compared with Examples 2 and 4, the tensile strength of the water-based clear paint prepared in Examples 5 to 6 is improved, and the time for bubbling to begin to appear when immersed in water at 40°C is increased, indicating that when the weight ratio of the hydroxyl acrylic resin to the water-based epoxy-modified acrylic resin is 3 to 7:1, the water resistance and mechanical properties of the water-based clear paint can be further improved.
[0046] Compared with Examples 6 to 7, the tensile strength of the water-based clear paint prepared in Examples 8 to 11 is improved, and the time for bubbling to begin to appear when immersed in water at 40°C is increased, indicating that when the hydroxy acrylic resin includes two hydroxy acrylic resins with different viscosities, the water resistance and mechanical properties of the water-based clear paint can be further improved. Compared with Examples 8 to 9, the tensile strength of the water-based clear paint prepared in Examples 10 to 11 is improved, and the time for bubbling to begin to appear when immersed in water at 40°C is increased, indicating that when the weight ratio of the first hydroxy acrylic resin to the second hydroxy acrylic resin is 3 to 4:2, the water resistance and mechanical properties of the water-based clear paint can be further improved. Compared with Example 11, the tensile strength of the water-based clear paint prepared in Examples 12 to 15 is improved, and the time for bubbling to begin to appear when immersed in water at 40°C is increased, indicating that the water resistance and mechanical properties of the water-based clear paint can be further improved by modifying the transparent powder using acrylonitrile-styrene-acrylate copolymer. In addition, compared with Examples 12 to 13, the tensile strength of the water-based clear paint prepared in Examples 14 to 15 is improved, and the time for bubbling to begin to appear when immersed in water at 40°C is increased, indicating that when the weight ratio of the transparent powder to the acrylonitrile-styrene-acrylate copolymer is 7 to 23:1, the water resistance and mechanical properties of the water-based clear paint can be further improved.
[0047] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A water-based clear paint, characterized in that: The composition comprises the following components in parts by weight: 30-50 parts of acrylic resin, 20-30 parts of transparent powder, 1-3 parts of dispersant, 1-2 parts of anti-settling agent, 0.5-1.5 parts of curing agent, 50 parts of water; The acrylic resin includes hydroxy acrylic resin and waterborne epoxy modified acrylic resin, and the weight ratio of the hydroxy acrylic resin to the waterborne epoxy modified acrylic resin is 1:9-9:
1.
2. A water-based clear paint according to claim 1, characterized in that: The weight ratio of the hydroxy acrylic resin to the waterborne epoxy modified acrylic resin is 3-7:
1.
3. A water-based clear paint according to claim 1, characterized in that: The hydroxy acrylic resin includes a first hydroxy acrylic resin and a second hydroxy acrylic resin, and the first hydroxy acrylic resin and the second hydroxy acrylic resin have different viscosities.
4. A water-based clear paint according to claim 3, characterized in that: The viscosity of the first hydroxy acrylic resin is 2800-4500 mPa·s, and the viscosity of the second hydroxy acrylic resin is 1400-2500 mPa·s.
5. A water-based clear paint according to claim 3, characterized in that: The weight ratio of the first hydroxy acrylic resin to the second hydroxy acrylic resin is 3-4:
2.
6. A water-based clear paint according to claim 1, characterized in that: The transparent powder is a modified transparent powder, and the raw materials of the modified transparent powder include transparent powder and acrylonitrile-styrene-acrylate copolymer.
7. A water-based clear paint according to claim 6, characterized in that: The weight ratio of the transparent powder to the acrylonitrile-styrene-acrylate copolymer is 7-23:
1.
8. A water-based clear paint according to claim 6, characterized in that: The preparation method of the modified transparent powder comprises the following steps: dissolving the acrylonitrile-styrene-acrylate copolymer in dimethylformamide to obtain an acrylonitrile-styrene-acrylate copolymer solution, adding the transparent powder into the acrylonitrile-styrene-acrylate copolymer solution, dispersing evenly, concentrating, and drying to obtain the modified transparent powder.
9. A water-based clear paint according to claim 1, characterized in that: The dispersant includes one or more of sodium oleate, polyvinyl alcohol, and sodium stearate; the anti-settling agent includes one or two of organic bentonite and fumed silica; and the curing agent includes one or two of water-based isocyanate and triethylenetetramine.
10. The method for preparing a water-based clear paint according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing and stirring the components in parts by weight to obtain a water-based transparent paint.
Citation Information
Patent Citations
Transparent waterborne woodware putty
CN105419448A
Water-based paint composition and preparation method thereof
CN105670441A
Water-based coating composition and method for producing multilayered coating film
JP2024018483A