High-scratch-resistance metal coating color-coated sheet and preparation method thereof
Through the combination of color primer + transparent topcoat and the use of materials such as silicon sol, polytetrafluoroethylene particles and polyurethane, the problem of poor scratch resistance of traditional metal-coated color-coated plates is solved, and a more uniform coating is achieved. Significantly improved scratch resistance and self-repair ability.
Patent Information
- Application Number
- CN202411412459.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional metal-coated color-coated plates have uneven coatings and easy scratches and wear problems in terms of scratches and wear, and the difference in density between primer and topcoat leads to uneven coatings, affecting the quality of the panel.
Using a combination of color primer + transparent topcoat, silicon sol and polytetrafluoroethylene particles are used as fillers, to improve the scratch resistance of the topcoat through nano-size effect and lubricating layer, and to add polyurethane and unsaturated poly to the topcoat Esters are used to enhance toughness and interface interactions, and surface coated with zinc chloride-ethanol solution to enhance self-healing capabilities.
Effectively reduce the uneven floating effect of color paste, improve the scratch resistance and self-repair ability of the topcoat, avoid the obvious contrast between the primer and the topcoat after scratches and wear, and enhance the wear resistance and resistance of the colored coated board. Scrape effect.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of color-coated plates, and more specifically, to a color-coated plate with a high scratch resistance metal coating and a preparation method thereof. Background Art
[0002] Metallic color-coated sheets are usually used in the fields of home appliance housings, rolling shutters, metal cabinets, building enclosures, etc. Traditional metal-coated anti-scratch color-coated sheets are painted with white primer + metallic topcoat containing anti-scratch particles. Due to the different densities of anti-scratch particles and color pastes, anti-scratch particles and metal powders are easy to precipitate, and the color paste floats on the surface. This oil-formulated paint and coating process easily cause the coating to form an uneven effect similar to cat paw prints, affecting the quality of the board surface. In addition, although the color-coated sheets after traditional painting are more wear-resistant and scratch-resistant than ordinary color-coated sheets, after friction with slightly hard and rough objects, they will leave obvious scratches and scratches, and the white primer will leak out. Therefore, it is necessary to further improve the anti-scratch effect of traditional metallic color-coated sheets. Summary of the invention
[0003] In order to improve the anti-scratch effect of metal color-coated plates, the present application provides a high-scratch-resistant metal coating color-coated plate and a preparation method thereof, adopting the following technical solutions: In a first aspect, the present application provides a highly scratch-resistant metal coating color-coated plate, comprising a metal substrate and a primer and a topcoat sequentially disposed on the same side surface of the metal substrate, wherein the primer comprises the following raw materials in parts by weight: Color paste 20-30 parts; Epoxy resin 40-60 parts; 0.5-1 part of leveling agent; 5-8 parts of isocyanate; 1-4 parts of n-butanol; 3-6 parts of DEB solvent; The topcoat comprises the following raw materials in parts by weight: Epoxy resin 30-40 parts; 20-30 parts of polyester resin; 5-8 parts of isocyanate; 0.5-1 part of leveling agent; 5-10 parts of filler; 1-4 parts of n-butanol; 3-6 parts of DEB solvent; 1 part of anti-settling agent; The filler includes silica sol and polytetrafluoroethylene particles.
[0004] By adopting the above technical solution, preferably using a combination of colored primer + transparent topcoat, the uneven effect of color paste floating on the surface to form a cat's paw print can be effectively reduced, and the filler in the topcoat can effectively improve the scratch resistance of the topcoat. Even if scratches and abrasions appear on the surface, there will be no obvious contrast between the leaked primer and the topcoat, and no obvious scratches and abrasions can be seen.
[0005] It is preferred to use silica sol and polytetrafluoroethylene particles as fillers. First, the addition of silica sol can cause entanglement between the topcoat and the polyester resin. The nano-size effect and large specific surface area of silica sol can be used to improve the interface interaction in the topcoat. When cracks are caused by scratches, the cracks are more susceptible to the passivation and obstruction of rigid particles when encountering nanoparticles, and then deflected and bifurcated, consuming more energy, effectively improving the toughness and scratch resistance of the topcoat. In addition, the addition of silica sol can also fill the plastic voids generated by the curing of epoxy resin, further improving the scratch resistance of the topcoat. The introduction of polytetrafluoroethylene particles can, on the one hand, fill the plastic voids generated by the topcoat during curing, and on the other hand, form a lubricating layer on the surface of the topcoat, forming an interlayer between the topcoat and the hard material to reduce the scratches caused by the hard material on the topcoat. In addition, when the filler is mixed, the polytetrafluoroethylene particles can also lubricate part of the silica sol, improve the dispersion effect and uniformity of the silica sol in the topcoat, so that the topcoat can obtain excellent lubricity and scratch resistance. The filler that falls off after scratching can lubricate the hard material or play a ball effect, thereby further improving the scratch resistance of the topcoat.
[0006] Optionally, the polyester resin includes polyurethane and unsaturated polyester.
[0007] By adopting the above technical scheme, preferably polyurethane and unsaturated polyester are added to the topcoat, the polyurethane and the unsaturated polyester can be bonded with each other, and the introduction of polyurethane can improve the toughness and interface wettability of the unsaturated polyester, which can not only form longer molecular chain segments in the topcoat to support and load the filler, reduce the sedimentation of the filler, and enable the filler to be evenly dispersed in the topcoat; it can also improve the bonding effect between the topcoat and the primer, reduce the possibility of the topcoat falling off, and enable the topcoat to stably protect the primer.
[0008] Optionally, the polyurethane is a coordination-modified polyurethane emulsion, and the unsaturated polyester resin is an unsaturated polyester resin containing pyridine.
[0009] Optionally, the polyurethane is prepared as follows: place polybutylene adipate in a container, heat, stir, add IPDI and DBTDL, continue to react, cool, add DMPA, continue to react, continue to cool, add DAP, react, add TEA, add deionized water, stir, and sonicate to obtain a polyurethane emulsion.
[0010] Optionally, the topcoat is also coated with a zinc chloride-ethanol solution.
[0011] By adopting the above technical scheme, it is preferred to apply zinc chloride-ethanol solution on the surface of the topcoat, and through the way of ion penetration, the zinc ions are infiltrated into the topcoat and coordinated with the coordination-modified polyurethane in the topcoat, and zinc-carboxyl and zinc-diaminopyridine bimetallic coordination structures can be formed, and the concentration of the coordination structure is sequentially reduced from the outside to the inside, and the bond energy of the strong coordination bond of zinc-diaminopyridine is much greater than the van der Waals force between molecules, so that the connection between molecules is tighter, and the surface of the topcoat can be hardened, and the scratch resistance of the topcoat can be further improved. At the same time, the weak coordination bond of zinc-carboxyl is highly reversible, and the bond energy is low, which is easier to break and reorganize, and effectively plays a role in fracture repair, so that the topcoat obtains an excellent self-repairing effect. In addition, since polyester is a polyester containing a pyridine structure, the metal ions can also form coordination with the pyridine group in the polyester resin, forming a stable cross-linked network in the topcoat, further improving the compactness and stability of the topcoat, so that the filler is stably located in the topcoat and is not easy to fall off, thereby improving the wear resistance and scratch resistance of the topcoat.
[0012] Optionally, the silica sol is selected from any one of silica sol SD-12040, silica sol SD-1430A, and silica sol SD-1430B.
[0013] By adopting the above technical solution, the particle size of the silica sol is optimized, and it can be evenly dispersed and filled in the pore structure of the topcoat at an appropriate addition amount, thereby evenly improving the hardness and scratch resistance of the topcoat.
[0014] Optionally, the silica sol is silica sol modified by a silane coupling agent.
[0015] By adopting the above technical solution, the silica sol is modified by a silane coupling agent, so that the dispersion of the silica sol in the topcoat is more uniform, and the occurrence of silica sol agglomeration is prevented, so that the silica sol can uniformly improve the hardness of the topcoat.
[0016] Optionally, the polytetrafluoroethylene particles include expanded polytetrafluoroethylene particles.
[0017] By adopting the above technical solution, some expanded polytetrafluoroethylene particles are selected and added to the topcoat, which can reduce the weight of the filler, making it more difficult for the filler to settle or float on the surface of the topcoat, which is conducive to the polytetrafluoroethylene particles forming a lubricating layer on the surface of the topcoat.
[0018] Optionally, the filler also includes polyethylene micro wax powder.
[0019] By adopting the above technical solution, preferably adding polyethylene micro wax powder to the topcoat, the pore structure formed by the topcoat and the primer can be further filled, the bonding effect between the topcoat and the primer can be improved, and the transparency of the topcoat can be improved, so that the topcoat can fully reveal the color effect of the primer.
[0020] In a second aspect, the present application provides a method for preparing a highly scratch-resistant metal coating color-coated plate, using the following technical solution: A method for preparing a highly scratch-resistant metal coating color-coated plate, S1, primer preparation: weighing a color paste, an epoxy resin, a leveling agent, an isocyanate, n-butanol and a DEB solvent respectively by weight, and mixing them to obtain a primer; S2, topcoat preparation: polyester resin, epoxy resin, leveling agent, isocyanate, filler, anti-settling agent, n-butanol and DEB solvent are weighed respectively by weight, and mixed to obtain a topcoat; S3. Preparation of color-coated plates: Clean the metal substrate and set it aside for use. Apply primer on the surface of the metal substrate. After drying, apply topcoat on the surface of the primer.
[0021] In summary, this application has the following beneficial effects: 1. Since the present application adopts a combination of colored primer + transparent topcoat, it can effectively reduce the uneven effect of color paste floating on the surface to form a cat's paw print, and the filler in the topcoat can effectively improve the scratch resistance of the topcoat. Even if scratches and abrasions appear on the surface, there will be no obvious contrast between the leaked primer and the topcoat, and no obvious scratches and abrasions can be seen. The nano-size effect and large specific surface area of silica sol are used to improve the interfacial interaction in the topcoat and fill the plastic voids generated by the curing of epoxy resin; the introduction of polytetrafluoroethylene particles can, on the one hand, fill the plastic voids generated by the topcoat during curing, and on the other hand, form a lubricating layer on the surface of the topcoat, forming an interlayer between the topcoat and the hard material to reduce the scratches caused by the hard material on the topcoat; 2. In the present application, polyurethane and unsaturated polyester are preferably added to the topcoat. The polyurethane and unsaturated polyester can be bonded to each other. The introduction of polyurethane can improve the toughness and interface wettability of the unsaturated polyester, and can not only form a longer molecular chain segment in the topcoat to support and load the filler, reduce the sedimentation of the filler, and enable the filler to be evenly dispersed in the topcoat; it can also improve the bonding effect between the topcoat and the primer, reduce the possibility of the topcoat falling off, and enable the topcoat to stably protect the primer; 3. The present application applies a zinc chloride-ethanol solution on the surface of the topcoat, and through ion penetration, the zinc ions penetrate into the topcoat and coordinate with the coordination-modified polyurethane in the topcoat, forming a zinc-carboxyl and zinc-diaminopyridine bimetallic coordination structure, and the concentration of the coordination structure decreases from the outside to the inside, hardening the surface of the topcoat. At the same time, the weak coordination bond of the zinc-carboxyl group is highly reversible, and the bond energy is low, which is easier to break and reorganize, effectively playing a role in fracture repair, so that the topcoat obtains an excellent self-repairing effect. In addition, since the polyester is a polyester containing a pyridine structure, the metal ions can also form a coordination with the pyridine group in the polyester resin, forming a stable cross-linked network in the topcoat, so that the filler is stably located in the topcoat and is not easy to fall off, thereby improving the wear resistance and scratch resistance of the topcoat. DETAILED DESCRIPTION
[0022] The present application is further described in detail below with reference to the embodiments.
[0023] Polyurethane Preparation Example Preparation Example 1 5mmol polybutylene adipate was placed in a container, heated to 110℃ and melted, sealed and stirred, the vacuum pump was turned on to remove moisture from the polyester, heated and maintained in vacuum, and when the reaction temperature dropped to 80℃, nitrogen was passed, 10.1mmol IPDI and 0.01g catalyst DBTDL were added dropwise, and the reaction was continued for 4h to obtain a transparent high-viscosity polyurethane prepolymer. The temperature was lowered to 70℃, 3mmol DMPA was added, and the reaction was continued for 2h, and when the temperature was lowered to 50℃, 2mmol DAP was added, and the reaction was continued for 2h, and TEA was added for neutralization, and the reaction was continued for 30min at room temperature to obtain a polyurethane emulsion.
[0024] Unsaturated polyester preparation example Preparation Example 2 Weigh 1,2-propylene glycol (PG), phthalic anhydride (PA), maleic anhydride (MA), and ligand 2,6-pyridinedicarboxylic acid (PDA) in a three-necked flask in a ratio of 1.1:0.5:0.3:0.2. The raw material alcohol-acid ratio is 1.1:1, and the ratio of saturated acid (PA+PDA) to unsaturated acid (MA) is 1:1. Add concentrated sulfuric acid as a catalyst in an amount of 0.1wt% of the dibasic acid. Pass nitrogen, stir and heat. When the temperature rises to 160°C, keep the temperature constant. After the steam temperature drops below 100°C, gradually increase the temperature to 190°C, continue the esterification reaction, and reach the theoretical water output. Connect a circulating water vacuum pump, keep the vacuum degree in the system at 0.1MPa, keep the temperature in the system constant, measure the acid value every half an hour, and the acid value will decrease as the reaction deepens. In order to ensure that the molecular weight of the unsaturated polyester meets the requirements, the acid value must be reduced to below 40mgKOH / g. After the polycondensation reaction was completed, a polymerization inhibitor, hydroquinone, was added in an amount of 0.5 wt % of the diol to obtain an unsaturated polyester prepolymer containing pyridine.
[0025] Preparation example of silica sol modified by silane coupling agent Preparation Example 3 Silica sol and silane coupling agent KH570 were taken in a mass ratio of 4:1, heated and stirred, refluxed, and distilled under reduced pressure to obtain modified silica sol.
[0026] Preparation Example of Zinc Chloride-Ethanol Solution Preparation Example 4 Zinc chloride is mixed with the ethanol solution to obtain a zinc chloride-ethanol solution with a mass fraction of 5%.
[0027] Example Examples 1-3 On the one hand, the present application provides a highly scratch-resistant metal coating color-coated plate, comprising a metal substrate and a primer and a topcoat sequentially arranged on the same side surface of the metal substrate; the primer comprises the following raw materials: color paste, epoxy resin, leveling agent, isocyanate, n-butanol, DEB solvent, as shown in the table below; the topcoat comprises the following raw materials: polyester resin, epoxy resin, leveling agent, isocyanate, n-butanol, DEB solvent, filler and anti-settling agent.
[0028] The polyester resin includes polyurethane and unsaturated polyester in equal amounts.
[0029] The filler includes silica sol and polytetrafluoroethylene particles of equal mass. The silica sol is silica sol SD-1430A. The leveling agent is BYK-371 leveling agent from Germany, the anti-settling agent is BYK-420 anti-settling agent from Germany, the color paste is Longsheng brand epoxy resin color paste LS-oil-based color paste, and the epoxy resin is E-44V epoxy resin produced by Langfang Nanze Anti-corrosion Materials Co., Ltd.
[0030] On the other hand, the present application provides a method for preparing a highly scratch-resistant metal coating color-coated plate, comprising the following steps: S1. Preparation of primer: weighing color paste, epoxy resin, leveling agent, isocyanate, n-butanol and DEB solvent respectively by weight, and mixing to obtain a primer; S2, topcoat preparation: polyester resin, epoxy resin, leveling agent, isocyanate, filler, anti-settling agent, n-butanol and DEB solvent are weighed respectively by weight, the filler is pre-grinded and mixed, and then mixed with other components to obtain a topcoat; S3. Preparation of color-coated plates: Clean the metal substrate and set it aside for use. Apply primer on the surface of the metal substrate. After drying, apply topcoat on the surface of the primer.
[0031] Table 1 Primer composition
[0032] Table 2 Topcoat composition
[0033] Example 4 The difference from Example 2 is that the polyester resin includes the polyurethane emulsion prepared in Preparation Example 1 and the polyester resin prepared in Preparation Example 2 in equal amounts.
[0034] In step S3, the surface of the topcoat in the preparation of the color-coated board is coated with the zinc chloride-ethanol solution prepared in Preparation Example 4, and dried to prepare the color-coated board.
[0035] Example 5 The difference from Example 2 is that the polytetrafluoroethylene particles include expanded polytetrafluoroethylene particles and polytetrafluoroethylene particles with a particle size of 70-90 μm of equal mass.
[0036] Example 6 The difference from Example 2 is that the silica sol in Example 2 is replaced by the silica sol modified by the silane coupling agent prepared in Preparation Example 3 with the same mass.
[0037] Example 7 The difference from Example 2 is that the filler includes silica sol, polytetrafluoroethylene particles and polyethylene micro wax powder in a mass ratio of 2:2:1.
[0038] Example 8 The difference from Example 4 is that the filler includes the silane coupling agent-modified silica sol prepared in Preparation Example 3, polytetrafluoroethylene particles, expanded polytetrafluoroethylene particles and polyethylene micro wax powder in a mass ratio of 2:1:1:1.
[0039] Comparative Example Comparative Example 1 The difference between this comparative example and Example 2 is that no polytetrafluoroethylene particles are added in this comparative example.
[0040] Comparative Example 2 The difference between this comparative example and Example 2 is that in this comparative example, the primer includes: 50kg epoxy resin, 0.7kg leveling agent, 5kg isocyanate, 1kg n-butanol and 3kg DEB solvent; the topcoat includes: 25kg color paste, 25kg polyester resin, 35kg epoxy resin, 0.7kg leveling agent, 5kg isocyanate, 1kg n-butanol, 3kg DEB solvent, 7kg filler and 1kg anti-settling agent.
[0041] Performance testing (1) Scratch resistance test: Scratch resistance test: According to the national standard "GB1768-(79)88 Paint film wear resistance test method", a JM-1 paint film wear tester is used. After a certain number of rotations, the weight loss of the paint film is used to indicate its wear resistance. (2) Repair test: Use the EXPERT model 3D surface profiler of the German BMT company to measure the cross-sectional area of the scratch notch (vertical measurement range 1mm, working distance 24mm, spot size 6μm, minimum step length 0.5μm, lateral resolution 30μm). Use a tool to make a scratch on the coating surface, and after being placed in a 60℃ forced air drying oven for 12 hours or placed at 60℃, 95%RH for 12 hours, use the instrument to measure the cross-sectional area after repair and calculate the self-repair efficiency; (3) Hardness test: Conduct pencil hardness test of coating film according to the provisions of GB / T6739-1996.
[0042] Table 3 Performance test
[0043] Combining the performance test comparison in Table 2, we can find that: 1. By comparing Examples 1-3 with Comparative Examples 1-2, it can be found that the scratch resistance of the color-coated plates prepared in Examples 1-3 is improved, which indicates that the combination of color primer + transparent topcoat in the present application can make the color-coated plates obtain a uniform surface state, and it is not easy to see obvious scratches after scratching. The introduction of silica sol, on the one hand, can entangle with macromolecules such as polyester resin, and utilize the nano-size effect and large specific surface area to improve the interface between the topcoat and the primer. When cracks are generated by scratching, the cracks are more susceptible to the passivation and obstruction of rigid particles when encountering nanoparticles, and then deflect and bifurcate, consuming more energy; on the other hand, it fills the plastic voids generated by the curing of epoxy resin, improves the density of the topcoat, and improves the wear resistance of the topcoat. The introduction of polytetrafluoroethylene particles can fill the plastic voids generated during the curing of the topcoat, and form a lubricating layer on the surface of the topcoat. The polytetrafluoroethylene particles can also lubricate part of the silica sol, improve the dispersion effect and uniformity of the silica sol in the topcoat, and make the topcoat have excellent lubricity and scratch resistance. The fillers dropped by scratching can lubricate hard materials or play a ball rolling effect, effectively improving the scratch resistance of the topcoat. 2. By comparing Example 4 with Example 2, it can be found that the scratch resistance and self-repairing effect of the color-coated plate prepared in Example 4 are improved. This means that in this application, zinc chloride-ethanol solution is coated on the surface of the topcoat, and zinc ions penetrate into the topcoat to form a zinc-carboxyl and zinc-diaminopyridine bimetallic coordination structure, forming an inner soft and outer hard structure to harden the surface of the topcoat. At the same time, the weak coordination bond of zinc-carboxyl is highly reversible, and the bond energy is low, which is easier to break and reorganize, and effectively plays a role in fracture repair, so that the topcoat obtains an excellent self-repairing effect. In addition, since polyester is a polyester containing a pyridine structure, the metal ions can also form coordination with the pyridine group in the polyester resin to form a stable cross-linked network in the topcoat, so that the filler is stably located in the topcoat and is not easy to fall off, thereby improving the wear resistance and scratch resistance of the topcoat; 3. By comparing Examples 5-6 with Example 2, it can be found that the scratch resistance of the color-coated plates prepared in Examples 5-6 is improved, which indicates that the addition of some expanded polytetrafluoroethylene particles to the topcoat in the present application can reduce the weight of the filler, making it more difficult for the filler to settle or float on the surface of the topcoat, which is conducive to the formation of a lubricating layer of polytetrafluoroethylene particles on the surface of the topcoat; 4. By comparing Examples 7-8 with Example 2, it can be found that the scratch resistance of the color-coated plates prepared in Examples 7-8 is improved, which means that in the present application, it is preferred to add polyethylene micro-wax powder to the topcoat, which can further fill the pore structure formed by the topcoat and the primer, improve the bonding effect between the topcoat and the primer, and also improve the transparency of the topcoat, so that the topcoat can fully reveal the color effect of the primer.
[0044] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A highly scratch-resistant metal coating color-coated sheet, characterized in that: It comprises a metal substrate and a primer and a topcoat sequentially arranged on the same side surface of the metal substrate, wherein the primer comprises the following raw materials in parts by weight: Color paste 20-30 parts; Epoxy resin 40-60 parts; 0.5-1 part of leveling agent; 5-8 parts of isocyanate; 1-4 parts of n-butanol; 3-6 parts of DEB solvent; The topcoat comprises the following raw materials in parts by weight: Epoxy resin 30-40 parts; 20-30 parts of polyester resin; 5-8 parts of isocyanate; 0.5-1 part of leveling agent; 5-10 parts of filler; 1-4 parts of n-butanol; 3-6 parts of DEB solvent; 1 part of anti-settling agent; The filler includes silica sol and polytetrafluoroethylene particles.
2. The highly scratch-resistant metal coating color-coated sheet according to claim 1, characterized in that: The polyester resin includes polyurethane and unsaturated polyester.
3. The highly scratch-resistant metal coating color-coated sheet according to claim 2, characterized in that: The polyurethane is a coordination-modified polyurethane emulsion, and the unsaturated polyester resin is an unsaturated polyester resin containing pyridine.
4. The highly scratch-resistant metal coating color-coated sheet according to claim 3, characterized in that: The preparation of the polyurethane is as follows: polybutylene adipate is placed in a container, heated, stirred, IPDI and DBTDL are added, the reaction is continued, the temperature is lowered, DMPA is added, the reaction is continued, the temperature is lowered, DAP is added, the reaction is continued, TEA is added, stirred, and ultrasonicated to obtain a polyurethane emulsion.
5. The highly scratch-resistant metal coating color-coated sheet according to claim 3, characterized in that: The topcoat is also coated with zinc chloride-ethanol solution.
6. The highly scratch-resistant metal coating color-coated sheet according to claim 1, characterized in that: The silica sol is selected from any one of silica sol SD-12040, silica sol SD-1430A and silica sol SD-1430B.
7. The highly scratch-resistant metal coating color-coated sheet according to claim 1, characterized in that: The silica sol is silica sol modified by a silane coupling agent.
8. The highly scratch-resistant metal coating color-coated sheet according to claim 1, characterized in that: The polytetrafluoroethylene particles include expanded polytetrafluoroethylene particles.
9. The highly scratch-resistant metal coating color-coated sheet according to claim 1, characterized in that: The filler also includes polyethylene micro wax powder.
10. The method for preparing a highly scratch-resistant metal coating color-coated plate according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Preparation of primer: weighing color paste, epoxy resin, leveling agent, isocyanate, n-butanol and DEB solvent respectively by weight, and mixing to obtain a primer; S2, topcoat preparation: polyester resin, epoxy resin, leveling agent, isocyanate, filler, anti-settling agent, n-butanol and DEB solvent are weighed respectively by weight, and mixed to obtain a topcoat; S3. Preparation of color-coated plates: Clean the metal substrate and set it aside for use. Apply primer on the surface of the metal substrate. After drying, apply topcoat on the surface of the primer.
Citation Information
Patent Citations
4-vinylpyridine resin and preparation method and application thereof
CN105693940A
Water-based self-repairing polyurethane coating based on metal coordination and preparation method of water-based self-repairing polyurethane coating
CN112920699A
Preparation process of high-hardness color-coated sheet and high-hardness color-coated sheet
CN115301519A
Inorganic zinc-rich coating for corrosion prevention of metal surface and preparation method of inorganic zinc-rich coating