High-wear-resistance durable non-stick ceramic coating as well as preparation method and coating method thereof

By using high wear-resistant, long-lasting non-stick ceramic coating formula and two-layer coating methods in ceramic coatings, the problem of easy decomposition and poor wear resistance at high temperatures is solved, and the high temperature non-decomposition and wear resistance are achieved Improvement, replacing fluorine coatings, meeting stricter safety and performance requirements.

CN119060629APending Publication Date: 2024-12-03FOSHAN SHUNDE DEFULONG NON-STICK COATING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411242174.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing ceramic coatings are easy to decompose under high temperature conditions, resulting in a decrease in non-stick properties and poor wear resistance, making it difficult to replace banned fluorine coatings, which poses food safety risks.

Method used

Using a high wear-resistant, long-lasting non-stick ceramic coating formula, including primer and topcoat, the combination of silica, modified nano-alumina, non-stick additives and other ingredients ensures that the coating film does not decompose at high temperatures and passes through The two-layer coating method of inner and outer layers improves the wear resistance and non-stickness of the coating.

Benefits of technology

The coating film does not decompose at high temperature of 500℃, significantly improves the wear resistance and non-stick durability of the coating, extends the product service life, and can not decompose below 320℃, replacing traditional fluorine coatings, satisfying stricter safety and performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060629A_ABST
    Figure CN119060629A_ABST
Patent Text Reader

Abstract

The invention discloses a durable non-stick ceramic coating with high wear resistance. The ceramic coating comprises a primer and a finish, the primer comprises the following components in terms of 100% of the total weight of the primer: 32-45% of a silicon dioxide solution; 19-25% of an inorganic pigment; 1-2% of a leveling agent; 1-2% of titanium powder; 18 to 28% of siloxane; 3 to 8 percent of isopropanol; 0.5 to 1.5 percent of glacial acetic acid; 5-8% of wear-resistant powder; 1-2% of a non-stick auxiliary agent; the finish paint comprises the following components in percentage by total weight of 100%: 43-55% of a silicon dioxide solution; 0-5% of an inorganic pigment; 1-2% of a leveling agent; 0-2% of titanium powder; 27% to 38.5% of siloxane; 3 to 8 percent of isopropanol; 1 to 1.5 percent of glacial acetic acid; 3-4% of wear-resistant powder; 2-4% of a non-stick auxiliary agent; the titanium powder, the wear-resistant powder, the non-stick additive and the like are added to physically coat polymethylsiloxane molecular groups, so that the wear resistance and the non-stick property of the surfaces of the polymethylsiloxane molecular groups are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a highly wear-resistant, durable and non-stick ceramic coating, a preparation method and a coating method thereof. Background Art

[0002] In the prior art, ceramic coatings usually adopt a composite structure of primer and topcoat. The primer is responsible for covering the substrate, corrosion resistance and wear resistance, etc., while the topcoat mainly provides non-stickiness and glossiness. However, the main components of conventional topcoats, such as polymethylsiloxane and silica, are prone to attenuation and decomposition under high temperature conditions, resulting in a continuous decrease in non-stick performance, which ultimately affects the service life and safety of the product and even poses a food safety risk. In addition, ceramic coatings in the prior art generally have problems such as low non-stick grade and poor wear resistance, making it difficult to replace fluorine-based coatings that are banned in the European Union and North America. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the present invention provides a highly wear-resistant and durable non-stick ceramic coating, a preparation method and a coating method thereof, which can significantly improve the non-stickiness and wear resistance of the coating to replace traditional fluorine coatings and meet more stringent safety and performance requirements.

[0004] The technical solution adopted by the present invention to solve its technical problem is:

[0005] A highly wear-resistant and durable non-stick ceramic coating, comprising a primer and a topcoat;

[0006] Based on 100% of the total weight of the primer, the primer includes:

[0007] Silica solution: 32-45%; Inorganic pigment: 19-25%; Leveling agent: 1-2%; Titanium powder: 1-2%; Siloxane: 18-28%; Isopropyl alcohol: 3-8%; Glacial acetic acid: 0.5-1.5%; Wear-resistant powder: 5-8%; Non-stick additive: 1-2%;

[0008] Based on 100% of the total weight of the topcoat, the topcoat includes:

[0009] Silica solution: 43-55%; Inorganic pigment: 0-5%; Leveling agent: 1-2%; Titanium powder: 0-2%; Siloxane: 27-38.5%; Isopropyl alcohol: 3-8%; Glacial acetic acid: 1-1.5%; Wear-resistant powder: 3-4%; Non-stick additive: 2-4%;

[0010] In some embodiments, the inorganic pigment is at least one of titanium dioxide, black iron oxide, red iron oxide, green iron oxide, yellow iron oxide, orange iron oxide, and brown iron oxide; the wear-resistant powder is modified nano-alumina of 3000 to 5000 mesh; and the non-stick additive is phenyl silicone oil.

[0011] A method for preparing a highly wear-resistant, durable, non-stick ceramic coating comprises the following steps:

[0012] (1) Preparation method of primer

[0013] Prepare component A: 32-45% silica solution, 19-25% inorganic pigment, 1-2% leveling agent, and 1-2% titanium powder are mixed in proportion and stirred for 30-120 minutes to ensure that there is no sediment;

[0014] Mixing of component B: Add 18-28% of siloxane, 1.2-5.5% of isopropyl alcohol, and 0.5-1.5% of glacial acetic acid to component A, and roll and ripen at a temperature of 5-35°C for 8-18 hours to allow them to fully react and dissolve each other, thereby obtaining a mixed solution of components AB;

[0015] Preparation of component C: Mix 1-2% of the non-stick additive, all the remaining isopropyl alcohol, and 5-8% of the wear-resistant powder, and completely disperse and refine them;

[0016] Add component C into the mixed solution of components AB and roll for 5 to 30 minutes to obtain the primer.

[0017] (2) Preparation method of topcoat

[0018] Prepare component A: 43-55% silica solution, 0-5% inorganic pigment, 1-2% leveling agent, and 0-2% titanium powder are mixed in proportion and stirred for 30-120 minutes to ensure that there is no sediment;

[0019] Mixing of component B: Add 27-38.5% of siloxane, 1.2-5.5% of isopropyl alcohol, and 1-1.5% of glacial acetic acid to component A, and roll and ripen at a temperature of 5-35°C for 8-18 hours to allow them to fully react and dissolve each other, thereby obtaining a mixed solution of components AB;

[0020] Preparation of component C: Mix 2-4% of the non-stick additive, all the remaining isopropyl alcohol, and 3-4% of the wear-resistant powder, and completely disperse and refine them;

[0021] Add component C into the mixed solution of components AB and roll for 5 to 30 minutes to obtain the topcoat.

[0022] A coating method for a highly wear-resistant, durable, non-stick ceramic coating comprises an inner and outer two-layer coating, wherein the bottom layer is a primer and the upper layer is a topcoat; the coating surface is smooth and glossy without protrusions and edges; the height difference between the highest point and the lowest point of the coating surface is 0.3 to 0.5 mm; and the edge R angle is set to R1 or R1.5 mm.

[0023] The beneficial effects of the present invention are:

[0024] 1. Non-decomposition property at high temperature: Compared with most polytetrafluoroethylene non-stick coatings on the market, the coating film made from the ceramic coating formula of the present invention does not decompose at a high temperature of 500°C, which is safer and healthier.

[0025] 2. Excellent coating wear resistance and coating non-stick durability: The coating film of this paint is not easily damaged. Even if the coating surface is damaged, the coating film still has good non-stick properties, which greatly extends the service life and usage experience of the product.

[0026] 3. Unlimited usage scenarios: When the coating film of this paint has a texture with a drop of more than 0.3mm on the surface of the substrate, it has extremely high wear resistance. The wear resistance test with a Meijie steel wool under a pressure of 2.5 kg can reach more than 20,000 times, which greatly extends the service life of the product.

[0027] 4. Can replace fluorine coating: The operating temperature is within 320℃, it does not decompose, and it is continuously non-sticky, which is 60℃ higher than the operating temperature of fluorine coating of 260℃, and can perfectly replace fluorine coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0029] Figure 1 is the molecular formula of polymethylsiloxane of the present application;

[0030] Figure 2 It is to add non-stick additives and wear-resistant powder to achieve the internal structure filling and wrapping schematic diagram;

[0031] Figure 3 It is a schematic diagram of the structure of the primer and topcoat of the present application;

[0032] Figure 4 This is a comparison table of high temperature non-decomposition tests of this application and fluorine coatings;

[0033] Figure 5 This is a test data table of non-stick coating wear resistance and non-stick coating long-lasting non-stick properties. DETAILED DESCRIPTION

[0034] First embodiment:

[0035] A method for preparing a highly wear-resistant, durable, non-stick ceramic coating comprises the following steps: (1) a method for preparing a primer;

[0036] Prepare component A: 32% silica solution, 19% inorganic pigment, 1.5% leveling agent, and 2% titanium powder are mixed in proportion and stirred for 30 minutes to ensure that there is no sediment;

[0037] Mixing of component B: Add 27% siloxane, 5.5% isopropyl alcohol and 0.5% glacial acetic acid to component A, roll and ripen at 5°C for 8 hours to allow them to fully react and dissolve each other, to obtain a mixed solution of components AB;

[0038] Prepare component C: mix 2% of the non-stick additive, all the remaining isopropyl alcohol, and 8% of the wear-resistant powder, and completely disperse and refine them;

[0039] Component C is added to the mixed solution of components AB, and the mixture is rolled for another 5 minutes to obtain a primer. In terms of weight percentage of the total weight of the primer, the isopropanol added in the above steps is 8% in total.

[0040] (2) Preparation method of topcoat

[0041] Prepare component A: 43% silica solution, 1% inorganic pigment, 2% leveling agent, and 2% titanium powder are mixed in proportion and stirred for 30 minutes to ensure that there is no sediment;

[0042] Mixing of component B: Add 38% siloxane, 5.5% isopropyl alcohol and 1% glacial acetic acid to component A, roll and ripen at 5°C for 8 hours to allow them to fully react and dissolve each other, to obtain a mixed solution of components AB;

[0043] Prepare component C: mix 2% of the non-stick additive, all the remaining isopropyl alcohol, and 3% of the wear-resistant powder, and completely disperse and refine them;

[0044] Component C is added to the mixed solution of components AB, and the topcoat is obtained after rolling for another 5 minutes. In terms of weight percentage of the total weight of the primer, the isopropanol added in all the above steps is 8%.

[0045] Second embodiment:

[0046] A method for preparing a highly wear-resistant, durable, non-stick ceramic coating comprises the following steps: (1) a method for preparing a primer;

[0047] Prepare component A: 37% silica solution, 21% inorganic pigment, 1.5% leveling agent, and 1.5% titanium powder are mixed in proportion and stirred for 80 minutes to ensure that there is no sediment;

[0048] Mixing of component B: Add 24% siloxane, 3% isopropyl alcohol and 1% glacial acetic acid to component A, roll and ripen at 20°C for 13 hours to allow them to fully react and dissolve each other, to obtain a mixed solution of components AB;

[0049] Prepare component C: mix 1.5% of the non-stick additive, all the remaining isopropyl alcohol, and 6% of the wear-resistant powder, and completely disperse and refine them;

[0050] Component C was added to the mixture of components AB, and the mixture was rolled for 13 minutes to obtain a primer. In terms of weight percentage of the total weight of the primer, the isopropanol added in the above steps was 6.5%.

[0051] (2) Preparation method of topcoat

[0052] Prepare component A: 49% silica solution, 2% inorganic pigment, 1.5% leveling agent, and 1.5% titanium powder are mixed in proportion and stirred for 20 minutes to ensure that there is no sediment;

[0053] Mixing of component B: Add 32.5% siloxane, 3% isopropyl alcohol and 1% glacial acetic acid to component A, roll and ripen at 20°C for 13 hours to allow them to fully react and dissolve each other, to obtain a mixed solution of components AB;

[0054] Prepare component C: mix 2% of the non-stick additive, all the remaining isopropyl alcohol, and 3% of the wear-resistant powder, and completely disperse and refine them;

[0055] Component C was added to the mixture of components AB, and the topcoat was obtained after rolling for 13 minutes. In terms of weight percentage of the total weight of the primer, the isopropanol added in the above steps was 6%.

[0056] Third embodiment:

[0057] A method for preparing a highly wear-resistant, durable, non-stick ceramic coating comprises the following steps: (1) a method for preparing a primer;

[0058] Prepare component A: 45% silica solution, 25% inorganic pigment, 1% leveling agent, and 1% titanium powder are mixed in proportion and stirred for 120 minutes to ensure that there is no sediment;

[0059] Mixing of component B: Add 17.5% siloxane, 1.2% isopropyl alcohol and 1.5% glacial acetic acid to component A, roll and ripen at 35°C for 18 hours to allow them to fully react and dissolve each other, to obtain a mixed solution of components AB;

[0060] Prepare component C: mix 1% of the non-stick additive, all the remaining isopropyl alcohol, and 5% of the wear-resistant powder, and completely disperse and refine them;

[0061] Component C is added to the mixed solution of components AB, and the mixture is rolled for 30 minutes to obtain a primer. In terms of weight percentage of the total weight of the primer, the isopropanol added in all the above steps is 3%.

[0062] (2) Preparation method of topcoat

[0063] Prepare component A: 54.5% silica solution, 5% inorganic pigment, and 1% leveling agent are mixed in proportion and stirred for 120 minutes to ensure that there is no sediment;

[0064] Mixing of component B: Add 27% siloxane, 1.2% isopropyl alcohol and 1.5% glacial acetic acid to component A, roll and ripen at 35°C for 18 hours to allow them to fully react and dissolve each other, to obtain a mixed solution of components AB;

[0065] Prepare component C: mix 4% of the non-stick additive, all the remaining isopropyl alcohol, and 4% of the wear-resistant powder, and completely disperse and refine them;

[0066] Component C is added to the mixed solution of components AB, and the topcoat is obtained after rolling for 30 minutes. In terms of weight percentage of the total weight of the primer, the isopropanol added in all the above steps is 3%.

[0067] The above examples 1 to 3 are calculated based on the weight percentage of each component in the total weight of the primer and topcoat. Details are shown in the following table:

[0068] Based on 100% total weight of primer Embodiment 1 Embodiment 2 Embodiment 3 Silica solution 32 37 45 Inorganic Pigments 19 21 25 Leveling agent 1.5 1.5 1 Titanium powder 2 1.5 1 Siloxane 27 24 17.5 Isopropyl alcohol 8 6.5 3 Glacial acetic acid 0.5 1 1.5 Wear-resistant powder 8 6 5 Non-stick additives 2 1.5 1 total 100 100 100

[0069] Based on 100% of the total weight of topcoat Embodiment 1 Embodiment 2 Embodiment 3 Silica solution 43 49 54.5 Inorganic Pigments 1 2 5 Leveling agent 2 1.5 1 Titanium powder 2 1.5 0 Siloxane 38 32.5 27 Isopropyl alcohol 8 6 3 Glacial acetic acid 1 1 1.5 Wear-resistant powder 3 3.5 4 Non-stick additives 2 3 4 total 100 100 100

[0070] Specifically, the inorganic pigment can be any one of titanium dioxide, black iron oxide, red iron oxide, green iron oxide, yellow iron oxide, orange iron oxide and brown iron oxide. The inorganic pigment provides the color of the coating, and the corresponding inorganic pigment is added according to the required color; titanium dioxide can be used for white, and black iron oxide and copper chromium black can be used for black; the wear-resistant powder is 3000-5000 mesh modified nano alumina, which can significantly improve the wear resistance of the coating, and the modified nano alumina produced by Shanghai Huijingya Nano New Materials Co., Ltd. can be used; the non-stick additive is phenyl silicone oil, which improves the non-stickiness of the coating surface by physical or chemical means; the leveling agent can improve the leveling of the coating surface by physical or chemical means, and the TEGO Glide4100 leveling agent can be used. Siloxane Si(CH3)4O3 is the main raw material for the formation of polymethylsiloxane, which has good high temperature resistance and chemical stability; silicon dioxide solution SiO2 reacts with siloxane to form methylsilane, which further participates in the polycondensation reaction to form a coating film; isopropyl alcohol C3H8O, as a solvent and reaction medium, promotes the polycondensation reaction; wear-resistant powder can significantly improve the wear resistance of the coating; titanium powder can improve the surface toughness and strength.

[0071] Reference Figure 1-Figure 5The present application physically coats polymethylsiloxane molecular groups by adding titanium powder, wear-resistant powder, non-stick additives, etc., thereby increasing the wear resistance and non-stick properties of the surface; at the same time, the preparation method and the coating method are designed and optimized to further enhance the wear resistance of the ceramic coating itself; the ceramic coating has strong comprehensive performance, which is mainly reflected in: non-stickiness and durability, and can still maintain a certain number of first-level non-stickiness under the action of external wear resistance, and the wear resistance and durability are significantly improved; it can replace conventional fluorine coatings, has a first-level non-stick grade, and has good wear resistance.

[0072] A coating method for a highly wear-resistant, durable, non-stick ceramic coating comprises an inner and outer two-layer coating, wherein the bottom layer is a primer and the upper layer is a topcoat; the coating surface is smooth and glossy without protrusions and edges; the height difference between the highest point and the lowest point of the coating surface is 0.3 to 0.5 mm; and the edge R angle is set to R1 or R1.5 mm.

[0073] Chemical reaction process and molecular formula:

[0074] 1. Reaction of siloxane and silicon dioxide:

[0075] 1. Reaction: In an acidic environment, siloxane (Si(CH3)4O3) reacts with silicon dioxide (SiO2) to produce methylsilane (CH3SiH3) and water (H2O).

[0076] 2. Simplified reaction formula: Si(CH3)4O3+SiO2→CH3SiH3+H2O

[0077] 2. Polycondensation reaction of methylsilane and isopropanol:

[0078] 1. Reaction: Methylsilane (CH3SiH3) undergoes a condensation reaction with isopropanol (C3H8O) under acidic conditions to generate cross-linked polymethylsiloxane.

[0079] 2. Polymethylsiloxane molecular formula: The molecular formula of polymethylsiloxane is usually expressed as [-(CH3)2SiO-]_n, where n represents the degree of polymerization, see Figure 1 shown.

[0080] These chemical reactions and formula designs together improve the wear resistance and non-stickiness of the coating, achieving the goal of replacing conventional fluorine coatings. The siloxane and silica solution react chemically in an acidic environment to generate methyl silane and water, and the methyl silane reacts with alcohols under acidic conditions to generate a cross-linked coating film.

[0081]

[0082] The polymethylsiloxane produced by polycondensation is a spiral chain polymer with large gaps between each methyl group. During the polycondensation reaction, a certain proportion of non-stick additives and wear-resistant powders are added to embed the non-stick additives and wear-resistant powders into the gaps between polymethylsiloxane molecules or wrap the outer surface of the methyl groups through the dispersion principle. In addition to its own non-stick and wear-resistant properties, polymethylsiloxane also has the properties of non-stick additives and wear-resistant powders, thereby improving the overall performance.

[0083] There are large gaps and spaces between the molecular clusters. By adding non-stick additives and wear-resistant powders, the internal structure is filled and wrapped. Figure 2 As shown. The non-stick additive is wrapped around the periphery of the methyl group, increasing the surface area of ​​the entire group. It plays a role in improving the non-stickiness of the surface. Wear-resistant powder molecules are embedded inside. When the coating is subjected to external extrusion friction, the wear-resistant group acts as a buffer between the polymethylsilane molecular groups, effectively reducing the friction between the molecular groups and delaying the life of the group. The wear-resistant molecules wrapped on the surface of the group enhance the wear resistance of the surface of the group, which can effectively reduce the consumption of the surface group and extend the life of the coating. After the internal reaction of the coating is completed, the coating process uses a two-layer coating method of inside and outside to paint the aluminum parts or die-castings. The bottom coating is called primer and the surface coating is called topcoat. See Figure 3 As shown, 5%-8% wear-resistant powder and 1%-2% non-stick additive are mainly added to the primer; 3-4% wear-resistant powder and 2-4% non-stick additive are added to the topcoat. By adding different proportions of wear-resistant powder to the primer and topcoat, two layers of coating with different hardness are formed; the topcoat has better flexibility and lower hardness; the primer has high hardness and a certain rigidity; the friction between the two bottom coatings is avoided when external force is applied, thereby improving the wear resistance. After adding the above proportion of non-stick additive to the primer, a certain non-stickiness can still be guaranteed when the topcoat is worn and the bottom is exposed. Refer to Figure 5 High wear resistance and durability means that after being rubbed 4500 to 5000 times with a scouring pad, or rubbed 5500 to 6500 times with a steel wool, it can still reach Level II.

Claims

1. A highly wear-resistant and durable non-stick ceramic coating. It is characterized in that Includes primer and topcoat; Based on 100% of the total weight of the primer, the primer includes: Silica solution: 32-45%; Inorganic pigment: 19-25%; Leveling agent: 1-2%; Titanium powder: 1-2%; Siloxane: 18-28%; Isopropyl alcohol: 3-8%; Glacial acetic acid: 0.5-1.5%; Wear-resistant powder: 5-8%; Non-stick additive: 1-2%; Based on 100% of the total weight of the topcoat, the topcoat includes: Silica solution: 43-55%; inorganic pigment: 0-5%; leveling agent: 1-2%; titanium powder: 0-2%; siloxane: 27-38.5%; isopropyl alcohol: 3-8%; glacial acetic acid: 1-1.5%; wear-resistant powder: 3-4%; non-stick additive: 2-4%.

2. A highly wear-resistant, durable, non-stick ceramic coating according to claim 1, Features: The inorganic pigment is at least one of titanium dioxide, black iron oxide, red iron oxide, green iron oxide, yellow iron oxide, orange iron oxide and brown iron oxide; the wear-resistant powder is modified nano-alumina with a mesh size of 3000 to 5000; and the non-stick additive is phenyl silicone oil.

3. A method for preparing a highly wear-resistant and durable non-stick ceramic coating. It is characterized in that The following steps are involved: (1) Preparation method of primer Prepare component A: 32-45% silica solution, 19-25% inorganic pigment, 1-2% leveling agent, and 1-2% titanium powder are mixed in proportion and stirred for 30-120 minutes to ensure that there is no sediment; Mixing of component B: Add 18-28% of siloxane, 1.2-5.5% of isopropyl alcohol, and 0.5-1.5% of glacial acetic acid to component A, and roll and ripen at a temperature of 5-35°C for 8-18 hours to allow them to fully react and dissolve each other, thereby obtaining a mixed solution of components AB; Preparation of component C: Mix 1-2% of the non-stick additive, all the remaining isopropyl alcohol, and 5-8% of the wear-resistant powder, and completely disperse and refine them; Add component C into the mixed solution of components AB and roll for 5 to 30 minutes to obtain the primer. (2) Preparation method of topcoat Prepare component A: 43-55% silica solution, 0-5% inorganic pigment, 1-2% leveling agent, and 0-2% titanium powder are mixed in proportion and stirred for 30-120 minutes to ensure that there is no sediment; Mixing of component B: Add 27-38.5% of siloxane, 1.2-5.5% of isopropyl alcohol, and 1-1.5% of glacial acetic acid to component A, and roll and ripen at a temperature of 5-35°C for 8-18 hours to allow them to fully react and dissolve each other, thereby obtaining a mixed solution of components AB; Preparation of component C: Mix 2-4% of the non-stick additive, all the remaining isopropyl alcohol, and 3-4% of the wear-resistant powder, and completely disperse and refine them; Add component C into the mixed solution of components AB and roll for 5 to 30 minutes to obtain the topcoat.

4. A coating method for a highly wear-resistant and durable non-stick ceramic coating, Features: Two layers of coating are used, the bottom layer is primer and the upper layer is topcoat; the coated surface is smooth and glossy without protrusions and edges, the height difference between the highest point and the lowest point of the coated surface is 0.3~0.5mm, and the edge R angle is set to R1 or R1.5mm.

Citation Information

Patent Citations

  • Titanium-containing ceramic paint and protective coating

    CN103013193A

  • Aqueous ceramic non-stick coating material for kitchenware surfaces and preparation method for aqueous ceramic non-stick coating material

    CN105778575A

  • Ceramic coating and preparation method thereof

    CN111073504A

  • Formula and process of Li porcelain iron pan coating

    CN113528008A

  • Enamel glaze inorganic non-stick coating material and application method thereof

    CN114479527A