Photovoltaic packaging adhesive film, preparation method thereof and photovoltaic module
By introducing reinforcing fibers into the photovoltaic packaging film and adopting melt extrusion granulation and casting molding processes, the problem of insufficient flexibility and buffering performance of the photovoltaic packaging film is solved, and the safety and lightweight components of the battery are improved. The impact resistance reduces production costs.
Patent Information
- Application Number
- CN202411232186.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
AI Technical Summary
The existing photovoltaic packaging films are insufficient in flexibility and buffering performance, resulting in high risk of cell cracking, and lightweight flexible photovoltaic modules have poor hail and impact resistance. It is necessary to develop shock-resistant photovoltaic packaging films to reduce risks and improve risks. ability.
By adopting the fiber-reinforced photovoltaic packaging film preparation method, the packaging film resin, reinforcement fiber, compatibility agent, antioxidant, etc. are mixed in a high-speed mixer, and then the double screw extrusion granulation and casting are prepared. Fiber-reinforced photovoltaic packaging film with improved buffering performance.
It effectively reduces the risk of cell cracking during packaging, and improves the hail and impact resistance of lightweight photovoltaic modules, while reducing production costs.
Smart Images

Figure CN119060639A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photovoltaic adhesive films, and in particular relates to a photovoltaic encapsulation adhesive film and a preparation method thereof, and a photovoltaic module. Background Art
[0002] Photovoltaic encapsulation film is a key material for the encapsulation of photovoltaic modules. It covers the upper and lower surfaces of the cells and is laminated with auxiliary materials such as the backplane in a vacuum environment to form photovoltaic modules. It mainly protects the cells and can effectively extend the service life of the modules. However, the EVA and POE particles commonly used in photovoltaic encapsulation films are relatively soft and have poor buffering properties. They cannot effectively reduce the risk of hidden cracks in the cells during the encapsulation process. In addition, lightweight flexible photovoltaic modules have poor hail and impact resistance compared to traditional glass modules and need to be reinforced with hard materials. Therefore, it is urgent to develop impact-resistant photovoltaic encapsulation films to reduce the risk of hidden cracks in the cells during the encapsulation process and improve the hail and impact resistance of lightweight modules.
[0003] Reinforcement fiber is glass fiber reinforced plastic and other composite materials used as structural materials, and is a commonly used fibrous reinforcement material. There are many types of reinforcement fibers, which can be roughly divided into two categories according to their chemical composition: inorganic fibers and organic fibers. Commonly used organic fibers are aramid fibers and nylon fibers, and commonly used inorganic fibers are glass fibers and carbon fibers. Among them, glass fiber is an inorganic non-metallic material with excellent performance and low price, and is usually used as a reinforcement material for composite materials. For example, the prior art uses a powdering process to prepare glass fiber reinforced PMMA (polymethyl methacrylate) photovoltaic packaging materials, which are widely used in the field of lightweight components. However, the powdering process requires a large investment in equipment, and the preparation of photovoltaic packaging materials is expensive. Therefore, it is urgent to develop a fiber-reinforced photovoltaic packaging material with a simple process and low price. Summary of the invention
[0004] Purpose of the invention: To achieve the above purpose, in view of the problems and shortcomings existing in the prior art, the present invention provides a method for preparing a fiber-reinforced photovoltaic encapsulation film, comprising the following steps:
[0005] S1, placing the encapsulating film resin, reinforcing fiber, compatibilizer and antioxidant in a high-speed mixer and mixing them evenly, and then extruding and granulating them using a twin-screw extruder to obtain a fiber-reinforced film resin special material;
[0006] S2, placing the fiber-reinforced film resin material obtained in S1, an initiator, a cross-linking agent, a tackifier, and an anti-ultraviolet additive in a high-speed mixer and mixing them evenly, and then extruding and casting to obtain the fiber-reinforced photovoltaic encapsulation film.
[0007] Furthermore, the encapsulation film resin of S1 includes any one of the following: EVA, POE, PVB. Before S1, the encapsulation film resin is first dried at 60-80° C. for 12-24 hours, and then cooled to room temperature by cold wind to obtain a dried encapsulation film resin.
[0008] Furthermore, the reinforcing fiber in S1 comprises any one or a combination of the following materials: carbon fiber, aramid fiber, glass fiber powder, short glass fiber filament, glass fiber winding, pultruded yarn, and the mass ratio of the packaging film resin to the reinforcing fiber is 90-40:10-60.
[0009] Furthermore, the compatibilizer in S1 includes any one or a combination of the following materials: EVA-g-MAH, EVA-g-GMA, POE-g-MAH, POE-g-GMA, and the addition ratio of the compatibilizer is 0.5wt% to 20wt% of the packaging film resin.
[0010] Furthermore, the initiator in S2 includes any one or a combination of the following materials: tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl peroxy (2-ethylhexyl) carbonate, diisopropyl peroxide, 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexane, tert-butyl peroxy 3,3,5-trimethylhexanoate, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxy isopropyl carbonate, and the initiator addition ratio is 0.3wt% to 2wt% of the encapsulation film resin.
[0011] Furthermore, the cross-linking agent in S2 includes any one or a combination of the following materials: triallyl isocyanurate, triallyl cyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, diethylene glycol dimethacrylate, and ethoxylated trimethylolpropane triacrylate, and the addition ratio of the cross-linking agent is 0.2wt% to 2wt% of the encapsulation film resin.
[0012] The tackifier in S2 includes any one or a combination of the following materials: γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-methacryloxypropyl, vinyltrimethoxysilane, and the addition ratio of the tackifier is 0.4wt% to 3wt% of the encapsulation film resin.
[0013] Further, the antioxidant includes any one or a combination of the following materials: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butylphenyl)phosphite, dilauryl thiodipropionate, N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate n-octadecyl alcohol, and the antioxidant is added in an amount of 0.1wt% to 3wt% of the encapsulation film resin;
[0014] The anti-ultraviolet auxiliary agent includes any one or a combination of the following materials: bisphenol A disalicylate, cyanuric chloride polymer, p-tert-octylphenyl salicylate, bis-2,2,6,6-tetramethylpiperidinol sebacate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-isooctyloxybenzophenone, and 2-hydroxy-4-methoxybenzophenone, and the addition ratio is 0.1wt% to 2wt% of the packaging film resin.
[0015] Furthermore, the temperature range of the twin-screw extrusion granulation in S1 is 100-180°C; the temperature range of the tape casting in S2 is 80-200°C.
[0016] On the other hand, the present invention provides a photovoltaic encapsulation film prepared by the above preparation method.
[0017] On the other hand, the present invention provides a photovoltaic module, which includes a transparent front panel, a first photovoltaic encapsulation film, a solar cell, a second photovoltaic encapsulation film, and a photovoltaic back panel in sequence along the light incident direction, and the first photovoltaic encapsulation film and the second photovoltaic encapsulation film are prepared using the above-mentioned preparation method.
[0018] Beneficial effects:
[0019] The present invention improves the buffering performance of the photovoltaic encapsulation film by introducing reinforcing fibers into the raw materials of the photovoltaic encapsulation film, such as EVA, POE and PVB, to enhance the performance, thereby reducing the risk of hidden cracks in the cell during the encapsulation process. In order to reduce production costs, the present invention uses a melt extrusion granulation method to blend the raw materials of the photovoltaic encapsulation film, such as EVA, POE, PVB, and reinforcing fibers, and adds a certain compatibilizer to solve the interface problem between the two, and then adds an initiator, a cross-linking agent and other auxiliary agents to extrude and form a film to prepare a fiber-reinforced photovoltaic encapsulation film to reduce the risk of hidden cracks in the cell during the encapsulation process and improve the hail and impact resistance of the soft photovoltaic module. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 A schematic diagram of a method for preparing a photovoltaic encapsulation film in an embodiment of the present invention. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in combination with embodiments.
[0022] As shown in the figure, this embodiment provides a method for preparing a photovoltaic encapsulation film, comprising the following steps:
[0023] S1, placing the encapsulating film resin, reinforcing fiber, compatibilizer and antioxidant in a high-speed mixer and mixing them evenly, and then extruding and granulating them using a twin-screw extruder to obtain a fiber-reinforced film resin special material;
[0024] S2, placing the fiber-reinforced film resin material obtained in S1, an initiator, a cross-linking agent, a tackifier, and an anti-ultraviolet additive in a high-speed mixer and mixing them evenly, and then extruding and casting to obtain the fiber-reinforced photovoltaic encapsulation film.
[0025] Furthermore, the encapsulation film resin of S1 includes any one of the following: EVA, POE, PVB. Before S1, the encapsulation film resin is first dried at 60-80° C. for 12-24 hours, and then cooled to room temperature by cold wind to obtain a dried encapsulation film resin.
[0026] Furthermore, the reinforcing fiber in S1 comprises any one or a combination of the following materials: carbon fiber, aramid fiber, glass fiber powder, short glass fiber filament, glass fiber winding, pultruded yarn, and the mass ratio of the packaging film resin to the reinforcing fiber is 90-40:10-60.
[0027] Preferably, the photovoltaic encapsulation film comprises the following components and the weight fraction of each component is:
[0028] 40-90 parts of encapsulation film resin, 10-60 parts of reinforcing fiber, 5-10 parts of compatibilizer, 0.3-2 parts of initiator, 0.2-2 parts of cross-linking agent, 0.4-3 parts of tackifier, 0.1-3 parts of antioxidant and 0.1-2 parts of ultraviolet light stabilizer.
[0029] Furthermore, the compatibilizer in S1 includes any one or a combination of the following materials: EVA-g-MAH, EVA-g-GMA, POE-g-MAH, POE-g-GMA, and the addition ratio of the compatibilizer is 0.5wt% to 20wt% of the packaging film resin.
[0030] Furthermore, the initiator in S2 includes any one or a combination of the following materials: tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl peroxy (2-ethylhexyl) carbonate, diisopropyl peroxide, 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexane, tert-butyl peroxy 3,3,5-trimethylhexanoate, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxy isopropyl carbonate, and the initiator addition ratio is 0.3wt% to 2wt% of the encapsulation film resin.
[0031] Furthermore, the cross-linking agent in S2 includes any one or a combination of the following materials: triallyl isocyanurate, triallyl cyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, diethylene glycol dimethacrylate, and ethoxylated trimethylolpropane triacrylate, and the addition ratio of the cross-linking agent is 0.2wt% to 2wt% of the encapsulation film resin.
[0032] The tackifier in S2 includes any one or a combination of the following materials: γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-methacryloxypropyl, vinyltrimethoxysilane, and the addition ratio of the tackifier is 0.4wt% to 3wt% of the encapsulation film resin.
[0033] Further, the antioxidant includes any one or a combination of the following materials: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butylphenyl)phosphite, dilauryl thiodipropionate, N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate n-octadecyl alcohol, and the antioxidant is added in an amount of 0.1wt% to 3wt% of the encapsulation film resin;
[0034] The anti-ultraviolet auxiliary agent includes any one or a combination of the following materials: bisphenol A disalicylate, cyanuric chloride polymer, p-tert-octylphenyl salicylate, bis-2,2,6,6-tetramethylpiperidinol sebacate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-isooctyloxybenzophenone, and 2-hydroxy-4-methoxybenzophenone, and the addition ratio is 0.1wt% to 2wt% of the packaging film resin.
[0035] Furthermore, the temperature range of the twin-screw extrusion granulation in S1 is 100-180°C; the temperature range of the tape casting in S2 is 100-200°C.
[0036] On the other hand, the present invention provides a photovoltaic encapsulation film prepared by the above preparation method.
[0037] On the other hand, the present invention provides a photovoltaic module, which includes a transparent front panel, a first photovoltaic encapsulation film, a solar cell, a second photovoltaic encapsulation film, and a photovoltaic back panel in sequence along the light incident direction, and the first photovoltaic encapsulation film and the second photovoltaic encapsulation film are prepared using the above-mentioned preparation method.
[0038] Beneficial effects:
[0039] The present invention improves the buffering performance of the photovoltaic encapsulation film by introducing reinforcing fibers into the raw materials of the photovoltaic encapsulation film, such as EVA, POE and PVB, to enhance the performance, thereby reducing the risk of hidden cracks in the cell during the encapsulation process. In order to reduce production costs, the present invention uses a melt extrusion granulation method to blend the raw materials of the photovoltaic encapsulation film, such as EVA, POE, PVB, and reinforcing fibers, and adds a certain compatibilizer to solve the interface problem between the two, and then adds an initiator, a cross-linking agent and other auxiliary agents to extrude and form a film to prepare a fiber-reinforced photovoltaic encapsulation film to reduce the risk of hidden cracks in the cell during the encapsulation process and improve the hail and impact resistance of the soft photovoltaic module.
[0040] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in combination with embodiments.
[0041] Embodiment 1:
[0042] A photovoltaic encapsulation film is prepared by the following steps:
[0043] (1) Dried ethylene-vinyl acetate copolymer (EVA) and ethylene-vinyl acetate grafted maleic anhydride (EVA-g-MAH) raw material resin, short glass fiber (particle size 10 microns, length 5 mm), tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester are placed in a high-speed mixer and mixed evenly, and then twin-screw extrusion granulation is performed to obtain a special material for glass fiber reinforced film resin; wherein the mass ratio of EVA to short glass fiber is 65:35; the addition amount of EVA-g-MAH is 10wt% of the EVA resin; the tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester is 0.2wt% of the EVA resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 minutes, the speed is 500rpm, and the temperature of the twin-screw extrusion granulation is 100-120°C;
[0044] (2) The glass fiber reinforced EVA granules, tert-butyl peroxy-2-ethylhexyl carbonate, trimethylolpropane trimethacrylate, γ-aminopropyl triethoxysilane and 2-hydroxy-4-methoxybenzophenone obtained in step (1) are placed in a high-speed mixer and mixed evenly, and then extruded and cast to obtain the glass fiber reinforced photovoltaic encapsulation film; wherein the amount of tert-butyl peroxy-2-ethylhexyl carbonate added is 0.5wt% of the EVA resin; the amount of trimethylolpropane trimethacrylate added is 2wt% of the EVA resin; the amount of γ-aminopropyl triethoxysilane added is 3wt% of the EVA resin; and the amount of 2-hydroxy-4-methoxybenzophenone added is 0.2wt% of the EVA resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 minutes, the speed is 600rpm, and the temperature of the extrusion casting molding is 80-120°C.
[0045] Embodiment 2:
[0046] A photovoltaic encapsulation film is prepared by the following steps:
[0047] (1) The dried ethylene-octene copolymer (POE) and ethylene-octene copolymer grafted maleic anhydride (POE-g-MAH) raw material resin, aramid fiber, and tris(2,4-di-tert-butylphenyl) phosphite are placed in a high-speed mixer and mixed evenly, and then twin-screw extrusion granulation is performed to obtain a fiber-reinforced film resin special material; wherein the mass ratio of POE to aramid fiber is 65:35; the addition amount of POE-g-MAH is 8wt% of the POE resin; tris(2,4-di-tert-butylphenyl) phosphite is 1wt% of the POE resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 20 minutes, the speed is 800rm, and the temperature of the twin-screw extrusion granulation is 100-120°C;
[0048] (2) The fiber-reinforced POE granules, tert-amyl peroxide (2-ethylhexyl) carbonate, triallyl isocyanurate, γ-(2,3-epoxypropoxy)propyl trimethoxysilane, and 2-hydroxy-4-isooctyloxybenzophenone obtained in step (1) are placed in a high-speed mixer and mixed evenly, and then extruded and cast to obtain the fiber-reinforced photovoltaic encapsulation film; wherein the amount of tert-amyl peroxide (2-ethylhexyl) carbonate added is 2wt% of the POE resin; the amount of triallyl isocyanurate added is 1.5wt% of the POE resin; the amount of γ-(2,3-epoxypropoxy)propyl trimethoxysilane added is 0.4wt% of the POE resin; the amount of 2-hydroxy-4-isooctyloxybenzophenone added is 2wt% of the POE resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 minutes, the speed is 700rm, and the temperature of the extrusion casting molding is 80-120°C.
[0049] Embodiment 3:
[0050] A photovoltaic encapsulation film is prepared by the following steps:
[0051] (1) placing dried ethylene-vinyl acetate copolymer (EVA) and ethylene-vinyl acetate grafted glycidyl methacrylate (EVA-g-GMA) raw material resins, glass fiber winding or pultruded yarn, and N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine in a high-speed mixer and mixing them evenly, and then extruding and granulating them using twin screws to obtain a special material for glass fiber reinforced film resin; wherein the mass ratio of EVA to short glass fiber is 40:60; the amount of EVA-g-GMA added is 10wt% of the EVA resin; the amount of N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine is 0.2wt% of the EVA resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 25 minutes, the speed is 1000 rm, and the temperature of the twin screw extrusion granulation is 100-120°C;
[0052] (2) The glass fiber reinforced EVA granules, tert-butyl hexanoate, trimethylolpropane triacrylate, γ-aminopropyl triethoxysilane and 2-hydroxy-4-methoxybenzophenone obtained in step (1) are placed in a high-speed mixer and mixed evenly, and then extruded and cast to obtain the glass fiber reinforced photovoltaic encapsulation film; wherein the amount of tert-butyl hexanoate added is 0.5wt% of the EVA resin; the amount of trimethylolpropane triacrylate added is 2wt% of the EVA resin; the amount of γ-aminopropyl triethoxysilane added is 3wt% of the EVA resin; and the amount of 2-hydroxy-4-methoxybenzophenone added is 0.2wt% of the EVA resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 25 minutes, the speed is 1000rm, and the temperature of the extrusion casting molding is 90-130°C.
[0053] Embodiment 4:
[0054] A photovoltaic encapsulation film is prepared by the following steps:
[0055] (1) The dried raw materials of ethylene-octene copolymer (POE) and ethylene-octene copolymer grafted with glycidyl methacrylate (POE-g-GMA), short glass fiber (particle size 10 μm, length 5 mm), and dilauryl thiodipropionate are placed in a high-speed mixer and mixed evenly, and then subjected to twin-screw extrusion granulation to obtain a fiber-reinforced film resin special material; wherein the mass ratio of POE to short glass fiber is 40:60; the amount of POE-g-GMA added is 10 wt% of the POE resin; the amount of dilauryl tetrathiodipropionate is 2 wt% of the POE resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 min, the speed is 1000 rm, and the temperature of the twin-screw extrusion granulation is 110-130° C.;
[0056] (2) The glass fiber reinforced POE granules, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, pentaerythritol triacrylate, vinyl trimethoxysilane and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole obtained in step (1) are placed in a high-speed mixer and mixed evenly, and then extruded and cast to obtain the glass fiber reinforced photovoltaic encapsulation film; wherein the amount of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane added is 2wt% of the POE resin; the amount of pentaerythritol triacrylate added is 1.5wt% of the POE resin; the amount of vinyl trimethoxysilane added is 0.4wt% of the POE resin; and the amount of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole added is 0.8wt% of the POE resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 minutes, the speed is 1000rm, and the temperature of the extrusion casting molding is 90-130°C.
[0057] Embodiment 5:
[0058] A photovoltaic encapsulation film is prepared by the following steps:
[0059] (1) The dried polyvinyl butyral (PVB) and EVA-g-MAH raw material resins, carbon fibers (surface plasma treated), and tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester are placed in a high-speed mixer and mixed evenly, and then twin-screw extrusion granulation is performed to obtain a fiber-reinforced film resin special material; wherein the mass ratio of PVB to carbon fibers is 80:20; the addition amount of EVA-g-MAH is 5wt% of the PVB resin; the addition amount of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester is 0.2wt% of the PVB resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 10 minutes, the speed is 800 rm, and the temperature of the twin-screw extrusion granulation is 100-120°C;
[0060] (2) The fiber-reinforced PVB granules, tert-butyl peroxy-2-ethylhexyl carbonate, trimethylolpropane trimethacrylate, γ-aminopropyl triethoxysilane and 2-hydroxy-4-methoxybenzophenone obtained in step (1) are placed in a high-speed mixer and mixed evenly, and then extruded and cast to obtain the fiber-reinforced photovoltaic encapsulation adhesive film; wherein the amount of tert-butyl peroxy-2-ethylhexyl carbonate added is 0.5wt% of the PVB resin; the amount of trimethylolpropane trimethacrylate added is 2wt% of the PVB resin; the amount of γ-aminopropyl triethoxysilane added is 3wt% of the PVB resin; and the amount of 2-hydroxy-4-methoxybenzophenone added is 0.2wt% of the PVB resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 minutes, the speed is 500rpm, and the temperature of the extrusion casting molding is 160-200°C.
[0061] Embodiment 6:
[0062] A photovoltaic encapsulation film is prepared by the following steps:
[0063] (1) The dried polyvinyl butyral (PVB) and EVA-g-GMA resin, aramid fiber, and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate are placed in a high-speed mixer and mixed evenly, and then twin-screw extrusion granulation is performed to obtain a special material for glass fiber reinforced film resin; wherein the mass ratio of PVB to aramid fiber is 40:60; the addition amount of EVA-g-MAH is 10wt% of the PVB resin; the addition amount of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate is 0.7wt% of the PVB resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 minutes, the speed is 1000rpm, and the temperature of the twin-screw extrusion granulation is 180-200°C;
[0064] (2) The fiber-reinforced PVB colloid particles, tert-butyl peroxyisopropyl carbonate, trimethylolpropane trimethacrylate, vinyl trimethoxysilane and tert-octylphenyl salicylate obtained in step (1) are placed in a high-speed mixer and mixed evenly, and then extruded and cast to obtain the fiber-reinforced photovoltaic encapsulation film; wherein the amount of tert-butyl peroxyisopropyl carbonate added is 0.7wt% of the PVB resin; the amount of trimethylolpropane trimethacrylate added is 1.5wt% of the PVB resin; the amount of vinyl trimethoxysilane added is 0.8wt% of the PVB resin; and the amount of tert-octylphenyl salicylate added is 0.35wt% of the PVB resin; the stirring conditions of the high-speed mixer are stirring at room temperature for 30 minutes at a speed of 500 rpm, and the temperature of the extrusion casting molding is 160-200°C.
[0065] Comparative Example 1:
[0066] EVA film is used as packaging material, and no impact-resistant layer material is added;
[0067] Comparative Example 2:
[0068] POE film is used as packaging material, and no impact-resistant layer material is added;
[0069] Preparation of lightweight flexible photovoltaic modules: stack a white or black back panel, a back packaging film, a battery layer, a front packaging film, and a transparent front panel in sequence from bottom to top, and laminate them into one piece using a laminator. The difference is that in the embodiment of the present invention, the back packaging film and the front packaging film are replaced with homemade glass fiber reinforced photovoltaic packaging film. In comparison example 1, the back and front packaging films are EVA films, respectively, and no impact-resistant layer material is added. In comparison example 2, the back and front packaging films are POE films, respectively, and no impact-resistant layer material is added!
[0070] Impact resistance test: An ice ball with a standard diameter of 25mm and a mass of 7.53g is launched at a speed of 23.0m / s to hit 11 positions of the packaged photovoltaic modules. The impact resistance of the photovoltaic modules is judged based on three requirements: appearance, maximum power attenuation and insulation resistance.
[0071] Film peel strength (with glass) test:
[0072] Take the fiber-reinforced photovoltaic encapsulation film prepared in Example 1, the EVA film of Comparative Example 1, the POE film of Comparative Example 2 300mm*300mm and the tempered glass 300mm*300mm*3.2mm and stack them in the order of glass / film / glass. Place the above samples in a laminator and heat to 100℃ and evacuate for 5 minutes, then pressurize to 0.5MPa and keep for 5 minutes; put them in a curing box and cross-link and cure them according to the curing temperature and time required by the product, then take them out and cool them to room temperature. Test its peel strength according to the GB / T 2790-1995 test standard!
[0073] Film peel strength (with back sheet) test:
[0074] Take the fiber reinforced photovoltaic encapsulation film prepared in the embodiment, the EVA film of comparative example 1, the POE film of comparative example 2 300mm*300mm and the backboard material of 310mm*310mm*0.3mm and stack them in the order of backboard / film / backboard. Place the above samples in a laminator, heat to 100°C and evacuate for 5 minutes, then pressurize to 0.5MPa and keep for 5 minutes; put them in a curing box for cross-linking and curing according to the curing temperature and time required by the product, then take them out and cool to room temperature. Test its peel strength according to the GB / T 2790-1995 test standard! The weather resistance test refers to testing the fiber reinforced photovoltaic encapsulation film, EVA film and POE film prepared in the embodiment of the present invention according to the IEC61215 and IEC61730 weather resistance test standards. The test results are shown in Table 1:
[0075] Table 1
[0076]
[0077] It can be seen from Table 1 that the glass fiber reinforced photovoltaic encapsulation film prepared in the embodiment of the present invention has no obvious defects in appearance after the impact test, the power attenuation is ≤5%, and the insulation resistance is ≥40MΩ.m 2 The peel strength with glass is ≥60N, and the peel strength with backboard material is ≥40N. The fiber-reinforced photovoltaic encapsulation film prepared by the present invention has low cost and no storage cycle problem. It can replace epoxy glass fiber prepreg and is widely used in the field of lightweight components.
[0078] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a photovoltaic encapsulation film, characterized in that: The following steps are involved: S1, placing the encapsulating film resin, reinforcing fiber, compatibilizer and antioxidant in a high-speed mixer and mixing them evenly, and then extruding and granulating them using a twin-screw extruder to obtain a fiber-reinforced film resin special material; S2, placing the fiber-reinforced film resin material obtained in S1, an initiator, a cross-linking agent, a tackifier, and an anti-ultraviolet additive in a high-speed mixer and mixing them evenly, and then extruding and casting to obtain a fiber-reinforced photovoltaic encapsulation film.
2. The method for preparing a photovoltaic encapsulation film according to claim 1, characterized in that: The packaging film resin of S1 includes any one of the following: EVA, POE, PVB. Before S1, the packaging film resin is first dried at 60-80° C. for 12-24 hours, and then cooled to room temperature by cold wind to obtain a dried packaging film resin.
3. The method for preparing a photovoltaic encapsulation film according to claim 1, characterized in that: The reinforcing fibers in S1 include any one or a combination of the following materials: carbon fiber, aramid fiber, glass fiber powder, short glass fiber filaments, glass fiber winding, pultruded yarn, and the mass ratio of the packaging film resin to the reinforcing fibers is 90-40:10-60.
4. The method for preparing a photovoltaic encapsulation film according to claim 1, characterized in that: The compatibilizer in S1 includes any one or a combination of the following materials: EVA-g-MAH, EVA-g-GMA, POE-g-MAH, POE-g-GMA, and the addition ratio of the compatibilizer is 0.5wt% to 20wt% of the packaging film resin.
5. The method for preparing a photovoltaic encapsulation film according to claim 1, characterized in that: The initiator in S2 includes any one or a combination of the following materials: tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl peroxy (2-ethylhexyl) carbonate, diisopropyl peroxide, 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexane, tert-butyl peroxy 3,3,5-trimethylhexanoate, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxy isopropyl carbonate, and the initiator addition ratio is 0.3wt% to 2wt% of the encapsulation film resin.
6. The method for preparing a photovoltaic encapsulation film according to claim 1, characterized in that: The cross-linking agent in S2 includes any one or a combination of the following materials: triallyl isocyanurate, triallyl cyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, diethylene glycol dimethacrylate, ethoxylated trimethylolpropane triacrylate or more, and the addition ratio of the cross-linking agent is 0.2wt% to 2wt% of the encapsulation film resin. The tackifier in S2 includes any one or a combination of the following materials: γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-methacryloxypropyl, vinyltrimethoxysilane, and the addition ratio of the tackifier is 0.4wt% to 3wt% of the encapsulation film resin.
7. The method for preparing a photovoltaic encapsulation film according to claim 1, characterized in that: The antioxidant comprises any one or a combination of the following materials: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butylphenyl)phosphite, dilauryl thiodipropionate, N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate n-octadecyl alcohol, and the antioxidant is added in an amount of 0.1wt% to 3wt% of the encapsulation film resin; The anti-ultraviolet auxiliary agent includes any one or a combination of the following materials: bisphenol A disalicylate, cyanuric chloride polymer, p-tert-octylphenyl salicylate, bis-2,2,6,6-tetramethylpiperidinol sebacate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-isooctyloxybenzophenone, and 2-hydroxy-4-methoxybenzophenone, and the addition ratio is 0.1wt% to 2wt% of the packaging film resin.
8. The method for preparing a photovoltaic encapsulation film according to claim 1, characterized in that: The temperature range of the twin-screw extrusion granulation in S1 is 100-180°C; the temperature range of the tape casting in S2 is 80-200°C.
9. A photovoltaic encapsulation film, characterized in that: The preparation method is described in any one of claims 1 to 8.
10. A photovoltaic module, characterized in that: The photovoltaic module includes a transparent front panel, a first photovoltaic encapsulation film, a solar cell, a second photovoltaic encapsulation film, and a photovoltaic back panel in sequence along the light incident direction. The first photovoltaic encapsulation film and the second photovoltaic encapsulation film are prepared using the preparation method described in any one of claims 1 to 8.