Colored packaging adhesive film and preparation method thereof
By orienting pigments parallel to the film plane through controlled heating and pressurizing, the method enhances color rendering and reduces pigment usage in colored encapsulation films, addressing high costs and poor color effects.
Patent Information
- Application Number
- CN202411396228.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-03
AI Technical Summary
Colored encapsulation films face issues of poor color rendering effect and high pigment usage, leading to increased costs.
A method involving heating and pressurizing a foaming material containing a matrix resin and pigment, controlling pressure and temperature to orient pigments parallel to the film plane, forming a dense pigment layer, thereby reducing pigment usage and enhancing color development.
Achieves high-quality color development with reduced pigment amounts, ensuring appearance performance and lowering production costs.
Smart Images

Figure CN119060651A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic module packaging films, and in particular to a colored packaging film and a preparation method thereof. Background Art
[0002] With the increasing promotion of photovoltaic modules, there is also a demand for personalized appearance, such as photovoltaic modules encapsulated with white packaging materials, black packaging materials, and colored packaging materials. This often requires adding fillers or pigments to the packaging materials to increase reflectivity or achieve the purpose of color adjustment. In recent years, colored photovoltaic films have been gradually used in the field of photovoltaic packaging as an emerging material. For example, white films can bring excellent reflective performance, which can effectively improve the photoelectric conversion efficiency and service life of the components, and play a key role in improving the efficiency and stability of photovoltaic systems. Black films can integrate the components with the appearance of the building, thereby improving the beauty and high-end feel of the component appearance, and are more popular in the household market. Colored packaging films are usually made by combining or dispersing specific color pigments (such as white titanium dioxide, calcium carbonate, black carbon black, and various colors of inorganic and organic pigments) in the film base, giving the film rich colors for various application scenarios. The cost of pigments is generally higher than that of base resins, and due to the large difference in polarity between pigments and film resins, the compatibility between the two is poor. It is usually necessary to add dispersants to improve the dispersion effect of fillers to improve the color rendering effect of the film. Even so, various types of colored encapsulation films still require the addition of more pigments to ensure the color rendering effect of the film. Therefore, colored encapsulation films currently face the problems of high pigment usage and high cost. Summary of the invention
[0003] The main purpose of the present invention is to provide a colored encapsulating adhesive film and a preparation method thereof, so as to solve the problems of poor color rendering effect, high pigment dosage and high cost of the colored encapsulating adhesive film in the prior art.
[0004] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a colored encapsulating film is provided, comprising the following steps:
[0005] The foaming material containing the matrix resin and the pigment is heated and pressurized to obtain a colored packaging film, the pressure of the heating and pressurizing treatment is not less than 2Mpa, the temperature T0 of the heating and pressurizing treatment satisfies T1-40≤T0, and T1 is the melting point temperature of the matrix resin.
[0006] Furthermore, the pressure of the heating and pressurizing treatment is 2Mpa to 10Mpa.
[0007] Preferably, the heating and pressurizing treatment includes a pre-pressing treatment and a pressure-maintaining treatment, and the steps of the heating and pressurizing treatment are as follows: the foaming material containing the matrix resin and the pigment is pre-pressurized at 4Mpa to 10Mpa, and then the pressure is released to 3Mpa to 5Mpa for pressure-maintaining treatment.
[0008] More preferably, the pre-pressing time is 1 min to 5 min, and the pressure-maintaining treatment time is 5 min to 10 min.
[0009] More preferably, the foaming material including the matrix resin and the pigment is laid flat in a thermoforming machine and subjected to heating and pressurizing treatment.
[0010] Furthermore, the temperature T0 of the heating and pressurizing treatment satisfies T1-40≤T0≤T1+40.
[0011] Preferably, the temperature T0 of the heating and pressurizing treatment satisfies: T1-10≤T0≤T1+10.
[0012] Furthermore, the foaming material containing a matrix resin and a pigment is selected from at least one of a foaming film containing a matrix resin and a pigment, foaming particles containing a matrix resin and a pigment, and a mixture of foaming particles containing a matrix resin and a pigment.
[0013] Furthermore, the foaming material comprising a matrix resin and a pigment is a foaming film comprising a matrix resin and a pigment; the foaming film comprising a matrix resin and a pigment is prepared by foaming through a physical method or a chemical method.
[0014] Furthermore, the adhesive film containing the matrix resin and the pigment and a physical foaming agent are added into a foaming kettle for physical foaming to obtain a foamed adhesive film containing the matrix resin and the pigment.
[0015] Preferably, the physical blowing agent is a supercritical fluid.
[0016] More preferably, the component of the supercritical fluid is selected from at least one of carbon dioxide, nitrogen and air.
[0017] More preferably, the film containing the matrix resin and the pigment is placed in a foaming kettle, the components of the supercritical fluid are introduced into the foaming kettle and heat and pressure are maintained under a supercritical state, and then the pressure is rapidly released to obtain a foamed film containing the matrix resin and the pigment.
[0018] More preferably, the temperature of the heat preservation and pressure holding treatment is T2, T1-10≤T2≤T1+10, wherein T1 is the melting point temperature of the matrix resin, and the time of the heat preservation and pressure holding treatment is 10 min to 30 min.
[0019] More preferably, when the component of the supercritical fluid is carbon dioxide, the pressure of the heat preservation and pressure preservation treatment is 7.5Mpa to 15Mpa.
[0020] More preferably, when the component of the supercritical fluid is nitrogen, the pressure of the heat preservation and pressure preservation treatment is 35Mpa to 40Mpa.
[0021] More preferably, the pressure relief time is ≤3s.
[0022] Furthermore, after the base resin, the pigment and the chemical foaming agent are mixed, the mixture is plasticized, extruded and cast into a film to obtain a foamed adhesive film containing the base resin and the pigment.
[0023] Preferably, the chemical foaming agent is selected from at least one of azodicarbonamide, azobisisobutyronitrile, barium azodicarboxylate, barium azodicarboxylate, dinitrosopentamethylenetetramine, trinitrosotrimethylenetriamine, 4,4-oxobisbenzenesulfonylhydrazide, benzenesulfonylhydrazide, 2,4-toluenedisulfonylhydrazide, oxalohydrazide, biurea, p-toluenesulfonylsemicarbazide, 2,4,6-trihydrazino-1,3,5-triazine, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, and sodium phosphite.
[0024] Preferably, the weight ratio of the base resin to the chemical foaming agent is (80-95):(1-3).
[0025] Furthermore, in the foaming material comprising a base resin and a pigment, a weight ratio of the base resin to the pigment is (80-99):(1-20).
[0026] Furthermore, the foaming material comprising a base resin and a pigment also includes a crosslinking agent, and the weight ratio of the base resin to the crosslinking agent is (80-95): (0.01-5), and the crosslinking agent is preferably selected from at least one of diisopropyl benzene peroxide, di(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and di(2,4-dichlorobenzoyl) peroxide.
[0027] Furthermore, the foaming material comprising a base resin and a pigment also includes a sensitizer, and the weight ratio of the base resin to the sensitizer is (80-95): (0.05-5), and the sensitizer is preferably selected from at least one of monoacyl phosphine, α-hydroxy ketone, diacyl phosphine, phenyl dimethyl ketal, 4-chlorobenzophenone, 2,4-diethylthioxanthone, phenyloxalyl ester, phenyloxalamide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-hydroxy-methylphenylpropane-1-one, and 6-isopropylferrocene (II) hexafluorophosphate.
[0028] Furthermore, the foaming material comprising a base resin and a pigment also includes a processing aid, and the weight ratio of the base resin to the processing aid is (80-95): (0-3). Preferably, the processing aid is selected from at least one of an antioxidant, a hindered amine light stabilizer, a UV absorber, and a plasticizer.
[0029] Furthermore, the matrix resin is selected from at least one of polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, acrylic resin, polysulfone, polyphenylene ether, ethylene vinyl acetate copolymer, ethylene octene copolymer, ethylene butene copolymer, polyvinyl formal, and epoxy resin.
[0030] Furthermore, the pigment is selected from at least one of inorganic pigments and organic pigments.
[0031] Preferably, the inorganic pigment is selected from at least one of white carbon black pigments, titanium dioxide pigments, calcium carbonate pigments, deuterium powder pigments, barium sulfate pigments, black carbon black pigments, iron chromium black pigments, chrome yellow pigments, molybdenum chrome red pigments, titanium yellow pigments, titanium brown pigments, cobalt blue pigments, cobalt green pigments, iron manganese black pigments, spinel black pigments, zinc sulfide pigments, molybdenum chrome red pigments, chrome green pigments, iron yellow pigments, iron brown pigments, ultramarine blue pigments, ultramarine violet pigments, and carbon nanotubes.
[0032] Preferably, the organic pigment is selected from at least one of acetylarylamide pigments, benzidine pigments, naphthol pigments, naphthol lake pigments, 2,3-acid pigments, 2,3-acid lake pigments, pyrazolone pigments, benzoxazolinone pigments, naphthol sulfonic acid pigments, pyrazoloquinazolinone pigments, quinacridone pigments, dioxazine pigments, 1,4-diketopyrrolopyrrole pigments, anthrone pigments, perylene pigments, pyrene pigments, anthracene lake pigments, triarylmethane pigments, triarylmethane lake pigments, nitro pigments, nitroso pigments, azomethine pigments, phthalocyanine pigments, azo pigments, isoindolinone pigments, and monoazo lake pigments.
[0033] Preferably, the particle size of the pigment is 0.01 μm to 100 μm.
[0034] According to another aspect of the present invention, a colored encapsulating adhesive film prepared by the above method for preparing a colored encapsulating adhesive film is provided.
[0035] By applying the technical solution of the present invention, a colored encapsulation film is prepared by heating and pressurizing a foaming material containing a matrix resin and a pigment, and controlling the pressure and temperature of the heating and pressurizing treatment, so that the bubbles in the matrix resin in a molten state collapse toward the plane of the film, and the pigment in the film is arranged around the bubbles as the bubbles collapse and tends to be arranged in a direction parallel to the plane of the film, forming a concentrated and dense pigment layer arrangement. The pigment layer concentrated and oriented around each bubble can achieve high-quality optical effects (for example, a high absorptivity or reflectivity to light), and at the same time can effectively reduce the amount of pigment added.
[0036] The preparation method of the colored packaging adhesive film of the present invention can not only achieve a high-quality color development effect to ensure the appearance performance of the adhesive film, but also effectively reduce the amount of pigment added and reduce the cost of the colored adhesive film. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0038] Figure 1 This is a SEM image of the foam film prepared in step 2 of Example 1;
[0039] Figure 2 This is a SEM image of the colored packaging film of the final product in Example 1. DETAILED DESCRIPTION
[0040] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0041] As described in the background art, the colored packaging film in the prior art has the problems of poor color rendering effect of the pigment of the colored packaging film, high pigment usage and high cost. In order to solve the above problems, according to one aspect of the present invention, a method for preparing a colored packaging film is provided, comprising the following steps:
[0042] The foaming material containing the matrix resin and the pigment is heated and pressurized to obtain a colored packaging film, the pressure of the heating and pressurizing treatment is not less than 2Mpa, the temperature T0 of the heating and pressurizing treatment satisfies T1-40≤T0, and T1 is the melting point temperature of the matrix resin.
[0043] In order to reduce the amount of pigment added and obtain a better color development effect, a colored encapsulating film is prepared by heating and pressurizing a foaming material containing a base resin and a pigment, and controlling the pressure and temperature of the heating and pressurizing treatment, so that the bubbles in the base resin in a molten state collapse in the direction of the film plane, and the pigment in the film is arranged around the bubbles along with the collapse of the bubbles and tends to be arranged in a direction parallel to the film plane, forming a concentrated and dense pigment layer arrangement, and the pigment layer concentrated and oriented around each bubble can achieve a high-quality optical effect (for example, a high absorptivity or reflectivity to light), and at the same time, the amount of pigment added can be effectively reduced. The preparation method of the colored encapsulating film of the present invention can not only achieve a high-quality color development effect to ensure the appearance performance of the film, but also effectively reduce the amount of pigment added and reduce the cost of the colored film.
[0044] In some embodiments, in order to obtain better coloring effect and reduce production energy consumption, the pressure of the heating and pressurizing treatment is 2Mpa~10Mpa; preferably, the heating and pressurizing treatment includes pre-pressing treatment and pressure holding treatment, and the steps of the heating and pressurizing treatment are as follows: the foaming material containing the matrix resin and the pigment is pre-pressurized at 4Mpa~10Mpa, and then the pressure is released to 3Mpa~5Mpa for pressure holding treatment; pre-pressing treatment is performed before the pressure holding treatment and then the pressure is released to a lower pressure for pressure holding treatment, which is conducive to the lateral collapse of the bubbles, the full orientation of the film and the pigment, and the adjustment of the thickness of the material, so as to prepare for the subsequent hot pressing process, so as to prepare a colored packaging film with uniform thickness and good coloring effect; preferably, the pre-pressing time is 1min~5min, and the pressure holding treatment time is 5min~10min; preferably, the foaming material containing the matrix resin and the pigment is spread flat in the hot pressing molding machine for heating and pressurizing treatment.
[0045] In some embodiments, the temperature T0 of the heating and pressurizing treatment satisfies T1-40≤T0≤T1+40; controlling the heating and pressurizing treatment to be within the above range is beneficial to the flow of the film so that the bubbles collapse toward the plane of the film and the pigments are oriented, and has lower production energy consumption; preferably, the temperature T0 of the heating and pressurizing treatment satisfies: T1-10≤T0≤T1+10.
[0046] In some embodiments, the foaming material comprising a matrix resin and a pigment is selected from at least one of a foaming film comprising a matrix resin and a pigment, foaming particles comprising a matrix resin and a pigment, and a mixture of foaming particles comprising a matrix resin and a pigment.
[0047] In some embodiments, the foaming material comprising a matrix resin and a pigment is a foamed film comprising a matrix resin and a pigment; the foamed film comprising a matrix resin and a pigment is prepared by foaming by a physical method or a chemical method. The inventor of the present application found that a film comprising a matrix resin and a pigment is first prepared, and then the film with the added pigment is processed by foaming, heating and pressing processes in sequence, and the growth of the pores in the foaming process is used to drive the polymer chains in the matrix resin to move and orient around the pores, which is conducive to driving the pigment to move and orient around the pores, and then the pigment in the matrix resin tends to be arranged in an orderly manner along a direction parallel to the film plane, and cooperates with the subsequent heating and pressing process to form an orderly and densely arranged reflective layer (e.g., a white pigment layer) or an absorption layer (e.g., a black pigment layer), thereby improving the color rendering effect.
[0048] In some embodiments, a film containing a matrix resin and a pigment and a physical foaming agent are added to a foaming kettle for physical foaming to obtain a foamed film containing a matrix resin and a pigment. The film containing a matrix resin and a pigment is used as a physical foaming object. In the foaming stage, the growth of the bubbles in the foaming process can be used to achieve the initial concentration and orientation of the pigment in the matrix resin, which is conducive to the subsequent heating and pressurization treatment of the pigment to further orient it to obtain a more concentrated and dense pigment layer, and the preparation process is simple; preferably, the physical foaming agent is a supercritical fluid. This system does not involve chemical reagent residues produced by chemical reactions. It is a more environmentally friendly foaming method and is conducive to the formation of a high pore density and a small-sized pore structure. The reaction is controllable, so that the subsequent heating and pressurization treatment can form a denser pigment layer and improve the color rendering effect; more preferably, the component of the supercritical fluid is selected from at least one of carbon dioxide, nitrogen, and air; more preferably, the film containing a matrix resin and a pigment is placed in a foaming kettle, and the components of the supercritical fluid are introduced into the foaming kettle and the foaming kettle is kept warm and pressurized under a supercritical state. The method further comprises the following steps: treating the supercritical fluid by heating and pressure-maintaining for 10 minutes to 30 minutes, and then rapidly releasing the pressure to obtain a foam film containing a matrix resin and a pigment; further preferably, the temperature of the heat preservation and pressure-maintaining treatment is T2, T1-10≤T2≤T1+10, wherein T1 is the melting point of the matrix resin, and the heat preservation and pressure-maintaining treatment time is 10 minutes to 30 minutes; further preferably, when the component of the supercritical fluid is carbon dioxide, the pressure of the heat preservation and pressure-maintaining treatment is 7.5 MPa to 15 MPa; further preferably, when the component of the supercritical fluid is nitrogen, the pressure of the heat preservation and pressure-maintaining treatment is 35 MPa to 40 MPa; further preferably, the pressure release time is ≤3 seconds, and by extremely rapid pressure release to normal pressure, an extremely high bubble nucleation rate is induced, which is conducive to the subsequent growth to form a bubble structure with a micro-nano size and a high pore density, so that a denser pigment layer can be formed by subsequent heating and pressure treatment, and the amount of pigment added can be effectively reduced.
[0049] In some embodiments, the matrix resin, the pigment and the chemical foaming agent are mixed, and then plasticized, extruded and cast into a film to obtain a foamed film containing the matrix resin and the pigment. The chemical foaming agent foams during the extrusion process, and the bubbles further grow and orient in the cast film, and drives the polymer chains in the matrix resin to move and orient around the bubbles, so that the pigment in the matrix resin tends to be arranged in an orderly manner along a direction parallel to the film plane, which is conducive to the formation of an orderly and densely arranged pigment layer with subsequent heating and pressure treatment; preferably, the chemical foaming agent is selected from azodicarbonamide, azobisisobutyronitrile, barium azodicarboxylate, barium azodicarboxylate, dinitrosopentamethylenetetramine, trinitrosotrimethylenetriamine, 4,4- At least one of oxybisbenzenesulfonyl hydrazide, benzenesulfonyl hydrazide, 2,4-toluene disulfonyl hydrazide, oxalohydrazide, biurea, p-toluenesulfonyl semicarbazide, 2,4,6-trihydrazino-1,3,5-triazine, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, and sodium phosphite; preferably, the weight ratio of the base resin to the chemical foaming agent is (80-95): (1-3), which is conducive to forming a cellular structure with micro-nano size and high pore density, so that a denser pigment layer can be formed by subsequent heating and pressure treatment, and at the same time, the amount of pigment added in the encapsulation film can be effectively reduced.
[0050] In order to ensure better color rendering effect while achieving lower cost, in some embodiments, in the foaming material including the base resin and the pigment, the weight ratio of the base resin to the pigment is (80-99): (1-20).
[0051] In some embodiments, the foaming material comprising a base resin and a pigment further includes a crosslinking agent, and the weight ratio of the base resin to the crosslinking agent is (80-95): (0.01-5), and the crosslinking agent is preferably selected from at least one of diisopropyl benzene peroxide, di(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and di(2,4-dichlorobenzoyl) peroxide.
[0052] In some embodiments, the foaming material comprising a base resin and a pigment further comprises a sensitizer, and the weight ratio of the base resin to the sensitizer is (80-95): (0.05-5), and the sensitizer is preferably selected from at least one of monoacyl phosphine, α-hydroxy ketone, diacyl phosphine, phenyl dimethyl ketal, 4-chlorobenzophenone, 2,4-diethylthioxanthone, phenyloxalyl ester, phenyloxalamide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-hydroxy-methylphenylpropane-1-one, and 6-isopropylferrocene (II) hexafluorophosphate.
[0053] In some embodiments, the foaming material comprising a base resin and a pigment also includes a processing aid, and the weight ratio of the base resin to the processing aid is (80-95): (0-3). Preferably, the processing aid is selected from at least one of an antioxidant, a hindered amine light stabilizer, a UV absorber, and a plasticizer.
[0054] In some embodiments, the matrix resin is selected from at least one of polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, acrylic resin, polysulfone, polyphenylene ether, ethylene vinyl acetate copolymer, ethylene octene copolymer, ethylene butene copolymer, polyvinyl formal, and epoxy resin. Of course, it can also be other polyolefins such as polybutene or copolymers of multiple olefins, or other thermoplastic resins suitable for preparing adhesive films in the prior art, which are not listed here one by one.
[0055] In some embodiments, the pigment is selected from at least one of inorganic pigments and organic pigments; preferably, the inorganic pigment is selected from at least one of white carbon black, titanium dioxide, calcium carbonate, de powder, barium sulfate, black carbon black, iron complex black, chrome yellow, molybdenum chrome red, titanium yellow, titanium brown, cobalt blue, cobalt green, iron manganese black, spinel black, zinc sulfide, molybdenum chrome red, chrome green, iron yellow, iron brown, ultramarine blue, ultramarine violet, and carbon nanotubes; preferably, the organic pigment is selected from at least one of acetylarylamide pigments, benzidine pigments, naphthol pigments, naphthol lake pigments, 2,3-acid pigments, 2,3-acid lake pigments, pyrazolone pigments, benzoxazolinone pigments, naphthol sulfonic acid pigments, pyrazoloquinazolinone At least one of pigments selected from the group consisting of quinacridone pigments, dioxazine pigments, 1,4-diketopyrrolopyrrole pigments, anthrone pigments, perylene pigments, pyrene pigments, anthracene lake pigments, triarylmethane pigments, triarylmethane lake pigments, nitro pigments, nitroso pigments, azomethine pigments, phthalocyanine pigments, azo pigments, isoindolinone pigments, and monoazo lake pigments; for example, the azo pigment may be an azo complex metal pigment, specifically a metal Ni complex azo pigment, such as CIPY150, CIPG10, and of course, it may also be an azo complex metal pigment formed by the complexation of other metals and azo, which are not listed here one by one. The isoindolinone pigment can be at least one of the metal Co and Ni complex isoindolinone pigments, such as CIPY177, CIPY179, CIPR257, and of course it can also be other metals and isoindolinone complex metal pigments formed by complexing, which are not listed here one by one. The monoazo lake pigment can be a monoazo barium salt lake pigment, such as CIPR48:1, CIPR49:1, CIPR51, CIPR53:1, CIPR57:2, and of course it can also be a monoazo lake pigment of other metal salts, which are not listed here one by one. The preferred particle size of the pigment is 0.01 μm to 100 μm, and the pigment particle size is within the above range, which is conducive to the orientation arrangement driven by pore growth, and the above smaller pigment particle size range is conducive to improving the tinting power, gloss, hiding power and weather resistance of the pigment.
[0056] According to another aspect of the present invention, a colored encapsulating adhesive film prepared by the above method for preparing a colored encapsulating adhesive film is provided.
[0057] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0058] Example 1
[0059] A method for preparing a colored packaging film comprises the following steps:
[0060] Step 1, film preparation: the matrix resin EVA (melting point of 80°C) and titanium dioxide (particle size of 0.5 μm) are mixed in a weight ratio of 95:5, and then plasticized, extruded and cast at 120°C to obtain a film;
[0061] Step 2, foaming treatment: placing the prepared film in a foaming kettle, then using a booster pump to introduce carbon dioxide supercritical fluid, the temperature in the foaming kettle is set to 80°C, the pressure in the foaming kettle is 10Mpa, and the temperature and pressure are maintained for 20 minutes and then the pressure is quickly released to obtain a foamed film;
[0062] Step 3: Heating and pressurizing treatment: Spread the prepared foam film in a hot pressing machine, set the temperature to 90°C, pre-press at 10 MPa for 3 minutes, then deflate to 4 MPa, and then maintain the pressure for 8 minutes to obtain a colored packaging film.
[0063] Example 2
[0064] A method for preparing a colored packaging film comprises the following steps:
[0065] Step 1, film preparation: base resin polyethylene (melting point 125°C) and white carbon black (particle size 0.8 μm) are mixed in a weight ratio of 99:1, and then plasticized, extruded and cast at 150°C to obtain a film;
[0066] Step 2, foaming: placing the prepared film in a foaming kettle, and then introducing carbon dioxide supercritical fluid using a booster pump, the temperature in the foaming kettle is set to 135°C, the pressure in the foaming kettle is 7.5Mpa, and the pressure is rapidly released after keeping the temperature and pressure for 10 minutes to obtain a foamed film;
[0067] Step 3: Heating and pressurizing treatment: Spread the prepared foam film in a hot pressing molding machine, set the temperature to 135°C, pre-press at a pressure of 4 MPa for 1 minute, then deflate to 3 MPa, and then maintain the pressure for 5 minutes to obtain a colored packaging film.
[0068] Example 3
[0069] A method for preparing a colored packaging film comprises the following steps:
[0070] Step 1, film preparation: base resin polyamide (melting point 260°C) and azo pigment (particle size 0.2 μm) CIPY150 are mixed in a weight ratio of 80:20, and then plasticized, extruded and cast at 280°C to obtain a film;
[0071] Step 2, foaming: the prepared film is placed in a foaming kettle, and then a supercritical fluid of carbon dioxide is introduced using a booster pump. The temperature in the foaming kettle is set to 250°C, and the pressure in the foaming kettle is 15Mpa. After maintaining the temperature and pressure for 30 minutes, the pressure is quickly released to obtain a foamed film.
[0072] Step 3: Heating and pressurizing treatment: Spread the prepared foam film flat in a hot pressing molding machine, set the temperature to 250°C, pre-press at a pressure of 10 MPa for 5 minutes, then deflate to 5 MPa, and then maintain the pressure for 10 minutes to obtain a colored packaging film.
[0073] Example 4
[0074] The only difference from Example 1 is that in step 1, the weight ratio of the matrix resin EVA to the titanium dioxide is 99:1.
[0075] Example 5
[0076] The only difference from Example 1 is that in step 1, the weight ratio of the matrix resin EVA to the titanium dioxide is 80:20.
[0077] Example 6
[0078] A method for preparing a colored packaging film comprises the following steps:
[0079] Step 1, film preparation: the matrix resin POE (melting point 80°C) and the carbon nanotubes (particle size 100nm) are mixed in a weight ratio of 93:2, and then plasticized, extruded and cast at 120°C to obtain a film;
[0080] Step 2, foaming: placing the prepared film in a foaming kettle, and then using a booster pump to introduce carbon dioxide supercritical fluid, the temperature in the foaming kettle is set to 80°C, the pressure in the foaming kettle is 10Mpa, and the temperature and pressure are maintained for 20 minutes and then the pressure is quickly released to obtain a foamed film;
[0081] Step 3: Heating and pressurizing treatment: Spread the prepared foam film flat in a hot pressing molding machine, set the temperature to 90°C, pre-press at 8 MPa for 3 minutes, then deflate to 5 MPa, and then maintain the pressure for 8 minutes to obtain a colored packaging film.
[0082] Example 7
[0083] A method for preparing a colored packaging film comprises the following steps:
[0084] Step 1, film preparation: base resin POE (melting point 80°C), carbon nanotubes (particle size 100nm) and chemical foaming agent dinitrosopentamethylenetetramine are mixed in a weight ratio of 93:2:2, and then plasticized and extruded at a high temperature of 120°C to obtain a foamed film;
[0085] Step 2: Heating and pressurizing treatment: Spread the prepared foam film flat in a hot pressing molding machine, set the temperature to 90°C, pre-press at 8 MPa for 3 minutes, then deflate to 5 MPa, and then maintain the pressure for 8 minutes to obtain a colored packaging film.
[0086] Example 8
[0087] A method for preparing a colored packaging film comprises the following steps:
[0088] Step 1: Foaming: Mix the matrix resin POE (melting point 80°C), carbon nanotubes (particle size 100nm) and chemical foaming agent dinitrosopentamethylenetetramine in a weight ratio of 93:2:2, and plasticize and extrude granules at a high temperature of 120°C to obtain foamed particles;
[0089] Step 2, compression molding: Spread the prepared foamed particles in a hot compression molding machine, set the temperature to 90°C, pre-press at 8 MPa for 3 minutes, then deflate to 5 MPa, and then maintain the pressure for 8 minutes to obtain a colored encapsulation film.
[0090] Example 9
[0091] A method for preparing a colored packaging film comprises the following steps:
[0092] Step 1: Foaming: Mix the matrix resin POE (melting point 80°C) and the chemical foaming agent dinitrosopentamethylenetetramine in a weight ratio of 95:2, and plasticize and extrude the mixture at a high temperature of 120°C to obtain foamed particles;
[0093] Step 2, compression molding: the prepared foamed particles and carbon black (particle size 600nm) are mixed in a weight ratio of 95:5 and spread flat in a hot pressing molding machine. The temperature is set to 90°C. After pre-pressing at a pressure of 8Mpa for 3min, the pressure is deflated to 5Mpa, and then the pressure is maintained for 8min to obtain a colored encapsulation film.
[0094] Example 10
[0095] A method for preparing a colored packaging film comprises the following steps:
[0096] Step 1, film preparation: the matrix resin POE (melting point is 80℃) and carbon nanotubes are mixed in a weight ratio of 95:5, and then spread on a hot press at 90℃, pre-pressed at a pressure of 8Mpa for 3min, then deflated to 5Mpa, and then maintained at a pressure of 8min to obtain a film;
[0097] Step 2, foaming treatment: placing the prepared film in a foaming kettle, then using a booster pump to introduce carbon dioxide supercritical fluid, the temperature in the foaming kettle is set to 80°C, the pressure in the foaming kettle is 10Mpa, and the temperature and pressure are maintained for 20 minutes and then the pressure is quickly released to obtain a foamed film;
[0098] Step 3: Heating and pressurizing treatment: Spread the prepared foam film flat in a hot pressing molding machine, set the temperature to 90°C, pre-press at 8 MPa for 3 minutes, then deflate to 5 MPa, and then maintain the pressure for 8 minutes to obtain a colored packaging film.
[0099] Embodiment 11
[0100] The only difference from Example 1 is that the temperature during the heating and pressurizing treatment is 40°C.
[0101] Example 12
[0102] The only difference from Example 1 is that the temperature during the heating and pressurizing treatment is 120°C.
[0103] Embodiment 13
[0104] The only difference from Example 1 is that the temperature of the heating and pressurizing treatment is 130°C.
[0105] Comparative Example 1
[0106] The only difference from Example 1 is that the holding pressure of the heating and pressurizing treatment is 0.5 MPa.
[0107] Comparative Example 2
[0108] The only difference from Example 1 is that the temperature of the heating and pressurizing treatment is 30°C.
[0109] Comparative Example 3
[0110] A method for preparing a colored packaging film comprises the following steps:
[0111] Step 1: Foaming treatment: Mix the matrix resin POE and the chemical foaming agent dinitrosopentamethylenetetramine in a weight ratio of 95:2, and plasticize and extrude the mixture at a high temperature of 120°C to obtain foamed particles;
[0112] Step 2, film casting: the prepared foamed particles and carbon black (particle size 600nm) are mixed in a weight ratio of 95:5, and then plasticized and extruded at a high temperature of 120°C to obtain a film;
[0113] Step 3: Heating and pressurizing treatment: Spread the prepared film flat in a hot pressing molding machine, set the temperature to 90°C, pre-press at 8 MPa for 3 minutes, then deflate to 5 MPa, and then maintain the pressure for 8 minutes to obtain a colored packaging film.
[0114] Comparative Example 4
[0115] A method for preparing a colored packaging film comprises the following steps:
[0116] The matrix resin EVA, titanium dioxide (particle size 0.5 μm) and EVA wax were mixed and granulated at a weight ratio of 80:15:5 at 120°C, and then plasticized, extruded and cast into a film at 90°C.
[0117] Comparative Example 5
[0118] A method for preparing a colored packaging film comprises the following steps:
[0119] The matrix resin EVA and titanium dioxide (particle size 0.5 μm) were mixed and granulated at a weight ratio of 95:5 at 120° C., and then plasticized, extruded and cast at 120° C. to obtain a colored encapsulation film.
[0120] Comparative Example 6
[0121] A method for preparing a colored packaging film comprises the following steps:
[0122] The base resin polyamide (melting point 260°C) and the azo pigment (particle size 0.2 μm) CIPY150 were mixed and granulated at a weight ratio of 80:20 at 280°C, and then plasticized, extruded and cast at 280°C to obtain a colored packaging film.
[0123] Comparative Example 7
[0124] A method for preparing a colored packaging film comprises the following steps:
[0125] The matrix resin POE (melting point 80°C) and carbon nanotubes (particle size 100nm) were mixed and granulated at a weight ratio of 93:2 at 120°C, and then plasticized, extruded and cast at 120°C to obtain a colored encapsulation film.
[0126] Performance Testing
[0127] The foaming film prepared in step 2 of Example 1 and the final product colored encapsulation film were characterized by SEM, and the results were as follows: Figure 1 and Figure 2 As shown. Figure 1 and Figure 2 It can be seen that the foamed film obtained by foaming treatment has a rich void structure, and the colored packaging film obtained by further heating and pressurizing treatment has an obvious layered structure.
[0128] Color rendering performance test: Referring to GB / T 5211.20-1999, the chromaticity values of the encapsulation films prepared in the examples and comparative examples were tested. The chromaticity values of the encapsulation films are shown in Table 1.
[0129] Performance test of light reflectivity and light transmittance of packaging film: The light reflectivity and light transmittance of the packaging films prepared in the embodiments and comparative examples were tested with reference to the following detection method. The detection method is as follows: Using a UV-visible spectrophotometer, a standard white board was taken for calibration, and then the transmittance and reflectivity of the packaging film in the wavelength range of 760 to 1100 nm were tested respectively. Three points were randomly tested and the average values were taken to obtain the reflectivity and transmittance. The reflectivity and transmittance data are specifically shown in Table 1.
[0130] Table 1
[0131] Chromaticity value (L) color Reflectivity(%) Light transmittance (%) Example 1 85 White 96 - Example 2 73 White 84 - Example 3 13 yellow - 8 Example 4 75 White 88 - Example 5 88 White 98 - Example 6 6 black - 6 Example 7 5 black - 3 Example 8 7 black - 7 Example 9 5 black - 3 Example 10 6 black - 6 Embodiment 11 67 White 80 - Example 12 84 White 94 - Embodiment 13 83 White 94 - Embodiment 14 83 White 93 - Comparative Example 1 64 White 78 - Comparative Example 2 51 White 53 - Comparative Example 3 8 black - 10 Comparative Example 4 82 White 92 - Comparative Example 5 62 White 77 - Comparative Example 6 19 yellow - 13 Comparative Example 7 10 black - 15
[0132] “-” means the relevant test was not performed.
[0133] It can be seen from Table 1 that the adhesive films prepared in Examples 1-13 of the present invention have excellent color development effects.
[0134] Compared with Comparative Examples 1-2 and Comparative Examples 4-5, the white pigment titanium dioxide in Example 1 has a higher reflectivity for visible light at 760-1100 nm and a better coloring (white) effect. Compared with Comparative Example 4, which uses a compatibilizer and increases the pigment content to improve the coloring effect, the white encapsulating film prepared in Example 1 still has a better coloring effect at a lower pigment content. Compared with Comparative Example 5, at the same pigment addition amount, the coloring effect of the white encapsulating film prepared in Example 1 is significantly improved.
[0135] Compared with Comparative Example 3 in which the foamed particles are subjected to sequential film casting and heating and pressurization treatment, Example 9 directly subjects the foamed particles of the matrix resin and the pigment to heating and pressurization treatment, which can avoid the pore structure being destroyed during the film casting process and making it impossible to carry out the subsequent heating and pressurization process of the pigment. The prepared black encapsulation film has lower light transmittance and better color rendering (black) effect.
[0136] Compared with Comparative Example 6, the yellow packaging film obtained by foaming, heating and pressurizing the film obtained by extrusion casting in Example 3 of the present invention has lower light transmittance and better color rendering (yellow) effect.
[0137] Compared with Comparative Example 7, the black packaging film obtained by foaming, heating and pressurizing the film obtained by extrusion casting in Example 6 of the present invention has lower light transmittance and better color rendering (black) effect.
[0138] Compared with Example 12 and Example 13, the light reflectivity of the white encapsulating film prepared in Example 1 is slightly higher, the color rendering (white) effect is slightly better, the temperature and pressure for preparing the encapsulating film are lower, and the energy consumption is lower;
[0139] Compared with Example 11, the white encapsulation film prepared in Example 1 has higher light reflectivity and better color rendering (white) effect.
[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a colored encapsulating film, It is characterized in that The process comprises the following steps: heating and pressurizing a foaming material containing a matrix resin and a pigment to obtain a colored encapsulating film, wherein the pressure of the heating and pressurizing treatment is not less than 2 MPa, and the temperature of the heating and pressurizing treatment is T 0 Meet T 1 -40≤T 0 , the T 1 is the melting point of the matrix resin.
2. The method for preparing the colored encapsulating film according to claim 1, It is characterized in that The pressure of the heating and pressurizing treatment is 2Mpa to 10Mpa; Preferably, the heating and pressurizing treatment includes a pre-pressing treatment and a pressure-maintaining treatment, and the steps of the heating and pressurizing treatment are as follows: the foaming material containing the matrix resin and the pigment is subjected to the pre-pressing treatment at 4Mpa to 10Mpa, and then the pressure is released to 3Mpa to 5Mpa for pressure-maintaining treatment; More preferably, the pre-pressing time is 1 min to 5 min, and the pressure holding time is 5 min to 10 min; More preferably, the foaming material comprising the matrix resin and the pigment is laid flat in the thermoforming machine for the heating and pressurizing treatment.
3. The method for preparing the colored encapsulating film according to claim 1, It is characterized in that The temperature of the heating and pressurizing treatment is T 0 Meet T 1 -40≤T 0 ≤T 1 +40; Preferably, the temperature of the heating and pressurizing treatment is 0 Satisfaction: T 1 -10≤T 0 ≤T 1 +10.
4. A method for preparing a colored encapsulating film according to any one of claims 1 to 3, It is characterized in that The foaming material containing a matrix resin and a pigment is selected from at least one of a foaming film containing a matrix resin and a pigment, foaming particles containing a matrix resin and a pigment, and a mixture of foaming particles containing a matrix resin and a pigment.
5. The method for preparing the colored encapsulating film according to claim 4, It is characterized in that The foaming material containing a matrix resin and a pigment is a foaming film containing a matrix resin and a pigment; the foaming film containing a matrix resin and a pigment is prepared by foaming through a physical method or a chemical method.
6. The method for preparing the colored encapsulating film according to claim 5, It is characterized in that Adding the adhesive film containing the matrix resin and the pigment and a physical foaming agent into a foaming kettle for physical foaming to obtain the foamed adhesive film containing the matrix resin and the pigment; Preferably, the physical foaming agent is a supercritical fluid; More preferably, the component of the supercritical fluid is selected from at least one of carbon dioxide, nitrogen and air; More preferably, the adhesive film comprising the matrix resin and the pigment is placed in the foaming kettle, a supercritical fluid component is introduced into the foaming kettle and heat and pressure are maintained under a supercritical state, and then the pressure is rapidly released to obtain the foamed adhesive film comprising the matrix resin and the pigment; More preferably, the temperature of the heat preservation and pressure preservation treatment is T 2 , the T 1 -10≤T 2 ≤T 1 +10, where the T 1 is the melting point temperature of the matrix resin, and the time of the heat preservation and pressure preservation treatment is 10min to 30min; More preferably, when the component of the supercritical fluid is carbon dioxide, the pressure of the heat preservation and pressure preservation treatment is 7.5Mpa to 15Mpa; More preferably, when the component of the supercritical fluid is nitrogen, the pressure of the heat preservation and pressure preservation treatment is 35Mpa to 40Mpa; More preferably, the pressure relief time is ≤3s.
7. The method for preparing the colored encapsulating film according to claim 5, It is characterized in that The base resin, the pigment and the chemical foaming agent are mixed, and then plasticized, extruded and cast into a film to obtain the foamed adhesive film containing the base resin and the pigment; Preferably, the chemical foaming agent is selected from at least one of azodicarbonamide, azobisisobutyronitrile, barium azodicarboxylate, barium azodicarboxylate, dinitrosopentamethylenetetramine, trinitrosotrimethylenetriamine, 4,4-oxobisbenzenesulfonylhydrazide, benzenesulfonylhydrazide, 2,4-toluenedisulfonylhydrazide, oxalohydrazide, biurea, p-toluenesulfonylsemicarbazide, 2,4,6-trihydrazino-1,3,5-triazine, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, and sodium phosphite; Preferably, the weight ratio of the base resin to the chemical foaming agent is (80-95):(1-3).
8. The method for preparing the colored encapsulating film according to claim 1, It is characterized in that In the foaming material comprising a base resin and a pigment, the weight ratio of the base resin to the pigment is (80-99): (1-20); and / or, The foaming material comprising a base resin and a pigment further comprises a crosslinking agent, wherein the weight ratio of the base resin to the crosslinking agent is (80-95): (0.01-5), and the crosslinking agent is preferably selected from at least one of dicumyl peroxide, di(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and di(2,4-dichlorobenzoyl)peroxide; and / or, The foaming material comprising a base resin and a pigment further comprises a sensitizer, wherein the weight ratio of the base resin to the sensitizer is (80-95):(0.05-5), and the sensitizer is preferably selected from at least one of monoacylphosphine, α-hydroxyketone, diacylphosphine, phenyl dimethyl ketal, 4-chlorobenzophenone, 2,4-diethylthioxanthone, phenyloxalyl ester, phenyloxalamide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-hydroxy-methylphenylpropane-1-one, and 6-isopropylferrocene (II) hexafluorophosphate; and / or, The foaming material comprising a base resin and a pigment further comprises a processing aid, wherein the weight ratio of the base resin to the processing aid is (80-95): (0-3), and the processing aid is preferably selected from at least one of an antioxidant, a hindered amine light stabilizer, an ultraviolet absorber, and a plasticizer; The matrix resin is selected from at least one of polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, acrylic resin, polysulfone, polyphenylene ether, ethylene vinyl acetate copolymer, ethylene octene copolymer, ethylene butene copolymer, polyvinyl formal, and epoxy resin.
9. The method for preparing the colored encapsulating film according to claim 1, It is characterized in that The pigment is selected from at least one of inorganic pigments and organic pigments; Preferably, the inorganic pigment is selected from at least one of white carbon black pigments, titanium dioxide pigments, calcium carbonate pigments, deuterium powder pigments, barium sulfate pigments, black carbon black pigments, iron chromium black pigments, chrome yellow pigments, molybdenum chrome red pigments, titanium yellow pigments, titanium brown pigments, cobalt blue pigments, cobalt green pigments, iron manganese black pigments, spinel black pigments, zinc sulfide pigments, molybdenum chrome red pigments, chrome green pigments, iron yellow pigments, iron brown pigments, ultramarine blue pigments, ultramarine violet pigments, and carbon nanotubes; Preferably, the organic pigment is selected from at least one of acetylarylamide pigments, benzidine pigments, naphthol pigments, naphthol lake pigments, 2,3-acid pigments, 2,3-acid lake pigments, pyrazolone pigments, benzoxazolinone pigments, naphthol sulfonic acid pigments, pyrazoloquinazolinone pigments, quinacridone pigments, dioxazine pigments, 1,4-diketopyrrolopyrrole pigments, anthrone pigments, perylene pigments, pyrene pigments, anthracene lake pigments, triarylmethane pigments, triarylmethane lake pigments, nitro pigments, nitroso pigments, azomethine pigments, phthalocyanine pigments, azo pigments, isoindolinone pigments, and monoazo lake pigments; Preferably, the particle size of the pigment is 0.01 μm to 100 μm. 10 . The colored encapsulating adhesive film prepared by the method for preparing a colored encapsulating adhesive film according to any one of claims 1 to 9.