Multifunctional adhesive with high-strength interface adhesion and chemical corrosion resistance

CN119060667APending Publication Date: 2024-12-03SHAANXI NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198026.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When conventional adhesives such as existing epoxy resin adhesives and polyurethane adhesives improve interface bonding performance and chemical corrosion resistance, they need to use volatile organic solvents to enhance interface wetting, resulting in limited environmental friendliness. , and it is difficult to meet the needs of high strength and multifunctional bonding.

Method used

Prepared by mixing imidazoles or pyridine ionic liquids with functional monomers without solvents, it forms a high-strength, chemical corrosion-resistant multifunctional adhesive with Good wetting and universality.

Benefits of technology

It realizes high-strength interface bonding, chemical corrosion resistance and environmentally friendly multifunctional bonding effect. The adhesive remains elastic at room temperature, can be stored stably for a long time, and maintains the bonding strength without attenuation under ultra-low temperature environment. It is suitable for A variety of materials, including metal, plastic and pine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060667A_ABST
    Figure CN119060667A_ABST
Patent Text Reader

Abstract

The invention discloses a multifunctional adhesive with high-strength interface adhesion and chemical corrosion resistance, which is prepared by mixing imidazole or pyridine ionic liquid with any one functional monomer of epoxy compound, aldehyde compound, anhydride, isocyanate and the like in a solvent-free manner. The adhesive is coated on a substrate material and is heated to generate a chemical reaction so as to be cured to generate a bonding effect. The adhesive disclosed by the invention has high-strength interface adhesiveness, high substrate adhesion adaptability and excellent chemical corrosivity and organic solvent tolerance, can realize efficient interface adhesion of materials such as metal, wood and polytetrafluoroethylene after being heated and cured, and still has relatively strong adhesion performance in an organic solvent or under a low-temperature or ultralow-temperature condition; the interface bonding can be stably maintained for a long time at an ultralow temperature (such as a liquid nitrogen environment) or in a plurality of organic solvents, and the bonding strength is not obviously attenuated in the process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface interface chemistry and interface bonding, and specifically relates to a multifunctional adhesive with high-strength interface bonding and chemical corrosion resistance, using imidazole or pyridine ionic liquid as a cross-linking curing agent. Background Art

[0002] Adhesive is a substance that is applied to the surface of two materials to achieve permanent or temporary bonding through the bonding process (Int. J. Adhes. Adhes., 2020, 98, 102530; The United States: William Andrew, 2011). The bonding process requires balancing the cohesive force between the adhesive molecules and the bonding force between the adhesive and the substrate to be bonded. Initially, people used animal bones and skins to make glue, which can bond the two together by producing a small surface chemical reaction. It can usually be used to connect metals, plastics, ceramics, cork, rubber and other materials, and can also be prepared into conductive materials (J. Mol. Liq., 2016, 220, 755-761; Compos. Part B-Eng., 2019, 163, 217-223; J. Alloy. Compd., 2019, 772, 912-919; Compos. Part B-Eng., 2017, 114, 299-310). Based on the adhesive bonding mechanism, adhesives are widely used in many fields including construction, packaging materials, aerospace, automobile manufacturing, biomedicine and textile industries. According to their sources and structural characteristics, adhesives are divided into natural adhesives and synthetic adhesives. Natural adhesives include bone glue, casein and protein adhesives and natural rubber adhesives. Synthetic adhesives can be further divided into four categories: acrylic, epoxy resin, silicone and polyurethane. Among them, epoxy resin adhesives in synthetic adhesives usually have excellent mechanical properties, high adhesion to many substrates, good heat resistance and chemical corrosion resistance, which have attracted people's attention. Therefore, they are widely used in various industries, such as construction, packaging materials, aerospace, automobile manufacturing, biomedicine and textile industries. With the increasing application fields, the requirements for functional adhesives such as epoxy resin adhesives, polyurethane adhesives, urea adhesives, and imines are also getting higher and higher, requiring not only high-strength bonding performance, but also excellent characteristics such as good environmental tolerance and substrate universality. However, conventional epoxy resin adhesives, polyurethane adhesives, urea adhesives, and imide adhesives usually require the participation of volatile substances such as organic solvents to increase the interfacial wettability of the adhesive, which is contrary to the principle of environmental friendliness. From the perspective of the curing mechanism of the adhesive, solving the wettability problem is the premise and basis for achieving efficient interfacial bonding of multifunctional adhesives. Summary of the invention

[0003] The purpose of the present invention is to provide a multifunctional adhesive which uses imidazole or pyridine ionic liquid as a crosslinking curing agent and has high-strength interface adhesion, high substrate adhesion adaptability and chemical corrosion resistance.

[0004] The multifunctional adhesive with high-strength interface adhesion and chemical corrosion resistance provided by the present invention is prepared by mixing imidazole or pyridine ionic liquid with functional monomers by solvent-free mixing; the imidazole or pyridine ionic liquid is composed of imidazolium ion or pyridinium ion and its corresponding anion, and the nitrogen atom of the imidazolium or pyridinium ion is connected with any one of an alkyl chain, an alkoxy chain, an alkyl chain with a hydrazide group or an amino group at the end, and an alkoxy chain with a hydrazide group or an amino group at the end; the anion is Cl - Br - ,I - 、NO3 - , [PF6] - 、[BF4]-、[Al2Cl7] - 、[AlCl4] - , [(CF3SO2)2N]-, dioctyl succinate sulfonate ion, [CF3SO3]-, [CF3COO]-; the functional monomer is selected from any one of epoxy compounds, aldehyde compounds, acid anhydrides, and isocyanates.

[0005] Furthermore, it is preferred that the ionic liquid is selected from any one of the following structural formulas:

[0006]

[0007] In the formula, m is an integer from 1 to 10, n is an integer from 1 to 10, and R1 represents Any of Represents anion.

[0008] Further, the epoxy compound is preferably selected from glycidyl phenyl ether, N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethylbiphenyl bisphenol diglycidyl ether, bisphenol A diglycidyl ether, 1,3-bis(oxiran-2-ylmethoxy)benzene, bisphenol F diglycidyl ether, 4-(diglycidylamino)phenyl glycidyl ether, 3,4-epoxycyclohexylmethyl-3,4-epoxy Any one or more of cyclohexyl carboxylate, di(3,4-epoxycyclohexylmethyl)hexanedioic acid, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, 1,3-bis[2-(3,4-epoxycyclohexyl)ethyl]tetramethyldisiloxane, glycidyl ether epoxycyclotetrasiloxane, epoxycyclohexylcyclotetrasiloxane, glycidyl ether oxypropyltrimethoxysilane, etc. In the present invention, the reaction of imidazole or pyridine ionic liquids with epoxy compounds involves the ring-opening process of epoxy groups. That is, when the ionic liquid contacts the epoxy compound, the nitrogen atom on the amino group will attack the epoxy group in the epoxy compound as a nucleophilic reagent, and the nitrogen atom will attack the carbon atom on the epoxy group. After the nucleophilic attack, the ethylene oxide (COC) ring of the epoxy compound will open to form an oxygen anion with a negative charge. The oxygen anion will obtain a proton from the proton donor to form a hydroxyl group (-OH). At this time, the reaction product is a derivative containing β-amino alcohol. The bonding and curing process of the epoxy compound in the present invention is essentially the result of a chemical cross-linking reaction induced by such a reaction.

[0009] Further, the aldehyde compound is preferably selected from 2,6-pyridinedicarboxaldehyde, 9,10-di(4-formylphenyl)anthracene, anthracene-9,10-dicarboxaldehyde, 2,5-dihydroxyterephthalaldehyde, 1,3,5-tri(3'-formyl-4'-hydroxybenzene)benzene, 1,3,5-tri(p-formylphenyl)benzene, 4,4',4"-[benzene-1,3,5-tri(acetylene-2,1-diyl)]tribenzaldehyde, 3,3',5,5'-tetra Any one or more of aldehyde-4,4'-dihydroxybiphenyl, isohexyl(4-aldehydephenyl)benzene, 4,4',4",4"',4"",4"-(9,10-dihydro-9,10-[1,2]benzanthracene-2,3,6,7,14,15-hexyl)benzaldehyde, [14'-[bis(3',5'-diformyl[1,1'-biphenyl]-4-yl)amino]-,1'-biphenyl]-3,5-dicarboxaldehyde, etc. In the present invention, the amino group (-NH2) in the imidazole or pyridine ionic liquid carries out a nucleophilic attack on the carbon atom in the aldehyde group (-CHO) in the aldehyde compound, the carbon-oxygen double bond (C=O) of the aldehyde group is destroyed, and the oxygen atom carries a negative charge to form an unstable hemiacetal intermediate. Afterwards, the oxygen anion obtains a proton from the nitrogen atom to form an intermediate with a hydroxyl group. Next, the proton on the hydroxyl oxygen atom is transferred to the nitrogen atom of the hydrazide, resulting in the elimination of water molecules, thereby forming a stable carbon-nitrogen double bond acylhydrazone bond (-CH=N-). The bonding and curing process of the aldehyde compound in the present invention is essentially the result of a chemical cross-linking reaction induced by such a reaction.

[0010] Further, it is preferred that the acid anhydride is selected from any one or more of tetrachlorophthalic anhydride, 1,8-naphthalene dicarboxylic anhydride, citraconic anhydride, 4,4'-biphenyl ether dianhydride, 4,4'-(hexafluoroisopropylene) dititanic anhydride, diethylenetriaminepentaacetic anhydride, 1,4,5,8-naphthalene tetracarboxylic anhydride, pyromellitic anhydride, 4,4'-oxydiphthalic anhydride, 3,3',4,4'-benzophenone tetracarboxylic anhydride, 4,4'-(4,4'-isopropyldiphenyloxy)bis(phthalic anhydride), etc. The reaction mechanism of imidazole or pyridine ionic liquids and acid anhydrides in the present invention varies with the change of reaction temperature. At low temperatures (usually below 100°C, room temperature or lower), the amino group first performs a nucleophilic attack on a carbonyl carbon in the acid anhydride, resulting in the opening of the acid anhydride ring. At high temperatures (above 100°C), imine compounds are formed along with the dehydration process. The bonding and curing process of the acid anhydride in the present invention is the result of a chemical cross-linking reaction induced by such reaction.

[0011] Further, the isocyanate is preferably selected from trimethylsilyl isocyanate, benzyl isocyanate, phenyl isothiocyanate, o-toluene isocyanate, toluene-2,4-isocyanate, m-phenyl-2,4-diisocyanate, 4,4'-methylenebis(phenyl isocyanate), isophorone diisocyanate, p-phenylene diisocyanate, 1,6-diisocyanato-2,2,4-trimethylhexane, diphenylmethane 4,4'-diisocyanate, hexamethylene diisocyanate. Any one or more of ester, m-xylene diisocyanate, 1,12-diisocyanato tridecane, 4-arm polyethylene glycol isocyanate, polyhexamethylene diisocyanate, polyhexamethylene diisocyanate, (4-isocyanate-phenoxy)-acetic acid 2-[2-(4-isocyanate-phenoxy)-acetoxy]-ethyl ester, 1,3,5-triisocyanate-2,4,6-trimethylbenzene, 3,3'-dimethyl-4,4'-biphenyl diisocyanate, etc. In the present invention, the reaction mechanism of imidazole or pyridine ionic liquids and isocyanates mainly involves the amino group performing nucleophilic attack on the isocyanate group (-N=C=O) in the isocyanate to generate a urea compound. That is, the amino group performs nucleophilic attack on the carbon atom in the isocyanate, resulting in the ring opening of the isocyanate group to generate a urea intermediate. In this process, the C=N bond of the isocyanate is opened, the amino group forms a new chemical bond with the carbon atom, and the nitrogen atom obtains a proton to form an intermediate with an amino group and a carbonyl group. Finally, this intermediate is stabilized by proton transfer and electron rearrangement to form a urea compound. The bonding and curing process of the isocyanate in the present invention is essentially the result of a chemical cross-linking reaction induced by such a reaction.

[0012] Furthermore, the molar ratio of the imidazole or pyridine ionic liquid to the functional monomer is 1:15 to 15:1, preferably the molar ratio of the imidazole or pyridine ionic liquid to the epoxy compound is 1:8 to 8:1, and preferably the molar ratio of the imidazole or pyridine ionic liquid to the aldehyde compound or acid anhydride or isocyanate is 1:5 to 5:1.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. The adhesive of the present invention has simple synthesis steps and cheap raw materials; each component of the adhesive is non-sticky and can be stored stably for a long time. The adhesive can be obtained after mixing and can be prepared as needed at any time.

[0015] 2. The adhesive of the present invention has good wettability and is green and environmentally friendly. It is a viscoelastic fluid dominated by elasticity at room temperature and has good universal applicability. It exhibits good bonding effects on a variety of materials such as stainless steel, iron, copper, aluminum, glass, PCTG (polyethylene terephthalate-1,4-cyclohexanedimethanol) plastic, ABS (terpolymer of acrylonitrile, butadiene and styrene) plastic and pine wood materials. The bonded samples can be separated as needed by heating or ethanol washing.

[0016] 3. The adhesive of the present invention can withstand organic solvents for a long time. The samples bonded by it have no obvious attenuation of bonding strength after being immersed in dozens of organic solvents such as dimethylformamide, acetonitrile, acetone, ethyl acetate, tetrahydrofuran, dichloromethane, anhydrous ether, toluene and n-hexane for a long time. The samples can be immersed for several months without falling off while carrying heavy objects.

[0017] 4. The adhesive of the present invention has good ultra-low temperature tolerance, maintains good stability when stored in ultra-low temperature environments such as liquid nitrogen (-196°C), and has no obvious attenuation of bonding strength, and has potential application value in the field of ultra-low temperature interface bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is the thermogravimetric graph of adhesive P1.

[0019] Figure 2 is a graph showing the variation of G' and G" with temperature for adhesives P1, P2, P3 and P4.

[0020] Figure 3 It is the graph of the complex viscosity of adhesives P1, P2, P3 and P4 as a function of temperature.

[0021] Figure 4 is the thermogravimetric graph of adhesive P2.

[0022] Figure 5 is the thermogravimetric graph of adhesive P3.

[0023] Figure 6 is the thermogravimetric graph of adhesive P4.

[0024] Figure 7 This is a digital photo of the adhesive P2 substrate universal hanging heavy objects display.

[0025] Figure 8 is the bond strength (MPa) of adhesive P1 to various substrates.

[0026] Fig. 9 is the bond strength (MPa) of adhesive P2 to various substrates.

[0027] Fig.10 This is a digital photo showing the solvent resistance of adhesive P2 hanging a heavy object.

[0028] Fig.11 is the adhesive strength (MPa) of adhesive P1 after immersion in various solvents for 30 days.

[0029] Fig.12 is the bond strength (MPa) of adhesive P2 after immersion in various solvents for 30 days.

[0030] Fig.13 is the bonding strength (MPa) of adhesive P1 tested in a liquid nitrogen environment.

[0031] Fig.14 is the bonding strength (MPa) of adhesive P2 tested in a liquid nitrogen environment.

[0032] Fig.15 is the adhesive strength (MPa) of adhesives B1, B2, and B3.

[0033] Fig.16 is the bonding strength (MPa) of adhesives C1, C2, and C3.

[0034] Fig.17 is the adhesive strength (MPa) of adhesives D1, D2, and D3. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to the following embodiments.

[0036] The specific structural formula of the imidazole ionic liquid used in the following examples is as follows:

[0037]

[0038]

[0039] Example 1

[0040] The imidazole ionic liquid represented by formula I-1 and glycidyl phenyl ether were fully ground and mixed in a molar ratio of 1:3 to obtain a translucent paste-like viscous substance, namely, adhesive P1. Figure 1 It can be seen that the thermal analysis decomposition temperature of adhesive P1 is ≥300℃, indicating that adhesive P1 is a viscoelastic complex fluid dominated by viscosity, and the storage modulus and loss modulus of adhesive P1 increase with the increase of frequency (see Figure 2), macroscopically, the liquid properties increase with increasing temperature, with the viscosity initially below 100°C and then reaching a plateau value. This phenomenon can be explained by the weakening of the non-covalent interactions between molecules in the adhesive; but when the temperature reaches 100°C, the adhesive viscosity continues to rise, and when it exceeds 110°C, the rate of increase accelerates sharply due to the curing process of the epoxy resin. In addition, when it exceeds 110°C, the storage modulus (G′) and loss modulus (G″) of the adhesive P1 both increase rapidly, the epoxy resin network begins to cross-link, the viscosity increases suddenly, and gelation or curing occurs (see Figure 3 ).

[0041] Example 2

[0042] The imidazole ionic liquid represented by formula I-2 and glycidyl phenyl ether were ground thoroughly at a molar ratio of 1:3 to obtain a translucent paste-like viscous substance, namely the adhesive P2. Figure 4 It can be seen that the thermal analysis decomposition temperature of adhesive P2 is ≥300°C, and its storage modulus (G′) is greater than the loss modulus (G″) (see Figure 2 ), which is a viscoelastic body dominated by elasticity on a macroscopic scale; when it exceeds 110°C, the storage modulus and loss modulus increase rapidly, the epoxy resin network begins to cross-link, the viscosity increases suddenly, and a curing phenomenon occurs (see Figure 3 ).

[0043] Example 3

[0044] The imidazole ionic liquid represented by formula I-3 and glycidyl phenyl ether were fully ground at a molar ratio of 1:3 to obtain a translucent paste-like viscous substance, namely, adhesive P3. Figure 5 It can be seen that the thermal analysis decomposition temperature of adhesive P3 is ≥300°C, and the storage modulus (G′) is greater than the loss modulus (G″) (see Figure 2 ), which is a viscoelastic body dominated by elasticity on a macroscopic scale; when the temperature exceeds 110°C, both the storage modulus and the loss modulus increase rapidly, the epoxy resin network begins to cross-link, the viscosity increases suddenly, and a curing phenomenon occurs (see Figure 3 ).

[0045] Example 4

[0046] The imidazole ionic liquid represented by formula I-4 and glycidyl phenyl ether were ground thoroughly at a molar ratio of 1:3 to obtain a translucent paste-like viscous substance, namely, the adhesive P4. Figure 6 It can be seen that the thermal analysis decomposition temperature of adhesive P4 is ≥300°C, and the storage modulus (G′) is greater than the loss modulus (G″) (see Figure 2 ), which is a viscoelastic body dominated by elasticity on a macroscopic scale; when the temperature exceeds 110°C, both the storage modulus and the loss modulus increase rapidly, the epoxy resin network begins to cross-link, the viscosity increases suddenly, and a curing phenomenon occurs (see Figure 3 ).

[0047] Example 5

[0048] The imidazole ionic liquid represented by formula I-5 and glycidyl phenyl ether were fully ground at a molar ratio of 1:3 to obtain a translucent paste-like viscous substance, namely, adhesive P1-1.

[0049] Example 6

[0050] The imidazole ionic liquid represented by formula I-6 and glycidyl phenyl ether were fully ground at a molar ratio of 1:3 to obtain a translucent paste-like viscous substance, namely, adhesive P1-2.

[0051] Example 7

[0052] The imidazole ionic liquid represented by formula I-1 and 2,6-pyridinedicarboxaldehyde were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive B1.

[0053] Example 8

[0054] The imidazole ionic liquid represented by formula I-1 and 9,10-di(4-formylphenyl)anthracene were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive B2.

[0055] Example 9

[0056] The imidazole ionic liquid represented by formula I-1 and anthracene-9,10-dicarboxaldehyde were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive B3.

[0057] Example 10

[0058] The imidazole ionic liquid represented by formula I-1 and toluene-2,4-isocyanate were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive C1.

[0059] Embodiment 11

[0060] The imidazole ionic liquid represented by formula I-1 and isophenyl-2,4-diisocyanate were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive C2.

[0061] Example 12

[0062] The imidazole ionic liquid represented by formula I-1 and 4,4'-methylenebis(phenyl isocyanate) were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive C3.

[0063] Embodiment 13

[0064] The imidazole ionic liquid represented by formula I-1 and tetrachlorophthalic anhydride were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive D1.

[0065] Embodiment 14

[0066] The imidazole ionic liquid represented by formula I-1 and 1,8-naphthalene dicarboxylic anhydride were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive D2.

[0067] Embodiment 15

[0068] The imidazole ionic liquid represented by formula I-1 and 4,4'-biphenyl ether dianhydride were fully ground at a molar ratio of 1:1 to obtain a translucent paste-like viscous substance, namely, adhesive D3.

[0069] The adhesive prepared in the above embodiment is tested for bonding performance. The interface materials used in the test are selected from metal materials such as 304 stainless steel (Steel), iron (Fe), aluminum (Al), copper (Cu), PCTG plastic, ABS plastic and pine wood materials. The test materials are all customized. The customized dimensions of metal materials such as 304 stainless steel, iron, aluminum, copper are 60mm long, 20mm wide and 3mm thick, while the thickness of plastic materials is 5mm. The strength of pine wood itself is relatively poor, with a thickness of 10mm. A circular hole with a diameter of 10mm is opened on one side of the interface material for hanging connection; the surface of the interface material is flat and has no deformation, and the edges are kept at right angles, which can ensure the reliability and repeatability of the test results. Taking metal materials such as 304 stainless steel as an example, the test method used for the bonding strength test is the lap shear test and the bonding area (200mm2) is strictly fixed. The test standard is based on GB / T 7124-2008 "Determination of tensile shear strength of adhesives". In order to achieve a better bonding effect and ensure the repeatability of bonding strength, the surface of the metal material needs to be polished. The grinding sandpaper is 600 mesh. After polishing, the metal powder on the surface of the material is wiped clean with lens paper. Then, the mixed adhesive is applied to the pair of clean metal sheets. The pair of metal sheets to be bonded are clamped and fixed with a long tail clip, placed in an oven for heating for 20 minutes, and cooled to room temperature to complete the interface bonding. A universal material testing machine (WDW-100M, Jinan Zhongluchang Testing Machine Company) is used for lap shear test. The test setting is a tensile shear rate of 5.0 mm min -1 , 7 parallel experiments were conducted in each group, and two extreme values ​​were removed. After the test, 5 experimental results were selected to calculate the average value as the final test result. Each group was plotted with the standard average deviation of 5 parallel experiments as the error bar. The stress per unit bonding area was calculated according to formula (1), which is the bonding strength of the sample.

[0070] T = F / S (1)

[0071] Where F is the peak stress at the moment of pulling apart, in N; S is the bonding area, in mm 2 ; T is the lap shear strength, unit is MPa.

[0072] like Figure 7 As shown, the adhesive P2 of Example 2 was used to bond 200 mm 2 304 stainless steel (Steel), iron (Fe), aluminum (Al) can easily bear 240kg weight, bonded copper (Cu) can bear 80kg weight, bonded pine can bear 20kg weight. Figure 8 and Fig. 9 It can be seen that adhesives P1 and P2 have strong bonding strength on various substrates.

[0073] Adhesive P1 of Example 1 and adhesive P2 of Example 2 were used to bond 200 mm thick 2 The 304 stainless steel samples were then immersed in organic solvents such as acetone, ethyl acetate, tetrahydrofuran, methylene chloride, anhydrous ether, toluene, and n-hexane for one month. Fig.10 It can be seen that the adhesive P2 is used to bond 200mm 2 304 stainless steel can still withstand a weight of 2.0kg after being soaked in organic solvents for a long time. Fig.11 and Fig.12 It can be seen that adhesives P1 and P2 are used to bond 200mm 2 After long-term immersion of 304 stainless steel in organic solvents, the bonding performance of the stainless steel samples did not significantly decay, and still showed a high bonding strength, which could be maintained at around 26.0MPa. However, in polar solvents such as ethanol, dimethylformamide, and acetonitrile, the bonding performance dropped to around 20.0MPa, and the bonding performance basically disappeared in water and methanol.

[0074] Adhesives P1 and P2 obtained in Example 1 and Example 2 were used to bond 200 mm thick 2 The 304 stainless steel samples were placed in a liquid nitrogen barrel (-196°C) to examine the change in adhesive strength over time. After the adhesives P1 and P2 were immersed in liquid nitrogen for 1, 3, 5, and 7 days, their bonding performance was significantly attenuated after the third day, but as time went on, the bonding strength was able to maintain a high value. The results are shown in Figure 2. Fig.13 and Fig.14 shown.

[0075] The adhesives of Examples 7 to 15 were used to bond 200 mm 2 The bond strengths of adhesives B1, B2, and B3 were 4.75 MPa, 4.42 MPa, and 8.69 MPa, respectively (see Fig.15 ), the bonding strengths of adhesives C1, C2, and C3 are 4.615MPa, 3.518MPa, and 8.947MPa, respectively (see Fig.16 ), the bonding strengths of adhesives D1, D2, and D3 are 4.308MPa, 5.019MPa, and 14.465MPa, respectively (see Fig.17 ).

[0076] Based on the above experimental results, it can be seen that the adhesive of the present invention exhibits good bonding effects on various materials such as 304 stainless steel, iron, aluminum, copper and other metal materials, as well as PCTG plastic, ABS plastic and pine wood materials, and can tolerate organic solvents. The bonding properties of the stainless steel samples bonded by the adhesive do not show obvious attenuation after being immersed in organic solvents such as acetone, ethyl acetate, tetrahydrofuran, dichloromethane, anhydrous ether, toluene, and n-hexane for one month, and still show high bonding strength. The adhesive does not fall off when immersed for several months while carrying heavy objects. The adhesive has good ultra-low temperature tolerance, maintains good stability in liquid gases such as liquid nitrogen, and has no obvious attenuation of its bonding strength when stored in a liquid nitrogen environment.

Claims

1. A multifunctional adhesive with high interfacial bonding and chemical resistance. It is characterized in that The adhesive is prepared by mixing imidazole or pyridine ionic liquid with functional monomers without solvent; The imidazole or pyridinium ionic liquid is composed of an imidazolium ion or a pyridinium ion and its corresponding anion, wherein the nitrogen atom of the imidazolium or pyridinium ion is connected to an alkyl chain, an alkoxy chain, an alkyl chain with a hydrazide or amino group at the end, or an alkoxy chain with a hydrazide or amino group at the end, and the anion is Cl - Br - 、I-、NO 3 - , [PF 6 ] - , [BF 4 ] - 、[Al 2 Cl 7 ] - 、[AlCl 4 ] - ,[(CF 3 SO 2 ) 2 N] - , dioctyl sulfosuccinate ion, [CF 3 SO 3 ] - , [CF 3 COO] - Any one of; The functional monomer is selected from any one of epoxy compounds, aldehyde compounds, acid anhydrides and isocyanates.

2. The multifunctional adhesive having high interfacial bonding and chemical corrosion resistance according to claim 1, It is characterized in that The ionic liquid is selected from any one of the following structural formulas: In the formula, m is an integer from 1 to 10, n is an integer from 1 to 10, and R 1 represent Any of Represents anion.

3. The multifunctional adhesive having high interfacial bonding and chemical corrosion resistance according to claim 1, It is characterized in that The epoxy compound is selected from the group consisting of glycidyl phenyl ether, N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethylbiphenyl bisphenol diglycidyl ether, bisphenol A diglycidyl ether, 1,3-bis(oxiran-2-ylmethoxy)benzene, bisphenol F diglycidyl ether, 4-(diglycidylamino)phenyl glycidyl ether, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexyl Any one or more of formate, di(3,4-epoxycyclohexylmethyl)adipic acid, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, 1,3-bis[2-(3,4-epoxycyclohexyl)ethyl]tetramethyldisiloxane, glycidyl ether epoxycyclotetrasiloxane, epoxycyclohexylcyclotetrasiloxane, and glycidyl ether oxygen propyl trimethoxysilane.

4. The multifunctional adhesive having high interfacial bonding and chemical corrosion resistance according to claim 1, It is characterized in that The aldehyde compound is selected from 2,6-pyridinedicarboxaldehyde, 9,10-di(4-formylphenyl)anthracene, anthracene-9,10-dicarboxaldehyde, 2,5-dihydroxyterephthalaldehyde, 1,3,5-tri(3'-formyl-4'-hydroxybenzene)benzene, 1,3,5-tri(p-formylphenyl)benzene, 4,4',4"-[benzene-1,3,5-tri(acetylene-2,1-diyl)]tribenzaldehyde, 3,3',5,5'-tetraformyl- Any one or more of 4,4'-dihydroxybiphenyl, isohexyl(4-formylphenyl)benzene, 4,4',4",4'',4''",4'',4''-(9,10-dihydro-9,10-[1,2]benzanthracene-2,3,6,7,14,15-hexyl)hexabenzaldehyde, and [14'-[bis(3',5'-diformyl[1,1'-biphenyl]-4-yl)amino]-,1'-biphenyl]-3,5-dicarboxaldehyde.

5. The multifunctional adhesive having high interfacial bonding and chemical corrosion resistance according to claim 1, It is characterized in that The acid anhydride is selected from any one or more of tetrachlorophthalic anhydride, 1,8-naphthalene dicarboxylic anhydride, citraconic anhydride, 4,4'-biphenyl ether dianhydride, 4,4'-(hexafluoroisopropylene) dititanic anhydride, diethylenetriaminepentaacetic dianhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride, pyromellitic anhydride, 4,4'-oxydiphthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic anhydride, and 4,4'-(4,4'-isopropyldiphenoxy)bis(phthalic anhydride).

6. The multifunctional adhesive having high interfacial bonding and chemical corrosion resistance according to claim 1, It is characterized in that The isocyanate is selected from trimethylsilyl isocyanate, benzyl isocyanate, phenyl isothiocyanate, o-toluene isocyanate, toluene-2,4-isocyanate, m-phenyl-2,4-diisocyanate, 4,4'-methylenebis(phenyl isocyanate), isophorone diisocyanate, p-phenylene diisocyanate, 1,6-diisocyanato-2,2,4-trimethylhexane, diphenylmethane 4,4'-diisocyanate, hexamethylene diisocyanate, m-phenylene diisocyanate, Any one or more of benzyl diisocyanate, 1,12-diisocyanatotridecane, 4-arm polyethylene glycol isocyanate, polyhexamethylene diisocyanate, polyhexamethylene diisocyanate, (4-isocyanate-phenoxy)-acetic acid 2-[2-(4-isocyanate-phenoxy)-acetoxy]-ethyl ester, 1,3,5-triisocyanate-2,4,6-trimethylbenzene, and 3,3'-dimethyl-4,4'-biphenyl diisocyanate.

7. The multifunctional adhesive having high interfacial adhesion and chemical corrosion resistance according to any one of claims 1 to 6, It is characterized in that The molar ratio of the imidazole or pyridine ionic liquid to the functional monomer is 1:15 to 15:

1.

8. The multifunctional adhesive having high interfacial bonding and chemical corrosion resistance according to claim 7, It is characterized in that The molar ratio of the imidazole or pyridine ionic liquid to the epoxy compound is 1:8 to 8:

1.