Yttrium titanate doped material, preparation method and application thereof

By doping silicon ions in yttrium titanate and preparing by sol-gel method, the problem of insufficient absorption performance of yttrium titanate material is solved, and higher electromagnetic wave absorption effect and feasibility of industrial production are achieved.

CN119060689APending Publication Date: 2024-12-03GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411175426.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing yttrium titanate materials and their dopants have poor performance in wave absorption performance and have failed to effectively absorb electromagnetic waves, especially in a wide frequency band, which has insufficient reflection loss and absorption bandwidth.

Method used

Y2Ti2-xSixO7 material is prepared by doping silicon ions in yttrium titanate, and prepared by sol-gel method to improve the absorbance performance of the material. The method includes stirring tetrabutyl titanate with ethanol citrate solution, adding a metal brine solution of ethyl orthosilicate and yttrium, heating through a water bath and oven heating to form a porous structure of yttrium titanate doped material.

Benefits of technology

It significantly improves the absorption performance of yttrium titanate material, achieves higher reflection loss and effective absorption bandwidth, is suitable for the absorbing coating of aircraft and electronic products, and reduces preparation energy consumption and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060689A_ABST
    Figure CN119060689A_ABST
Patent Text Reader

Abstract

The invention relates to the field of new materials, and discloses a yttrium titanate doped material, a preparation method and application thereof, and the preparation method comprises the following preparation steps: (a) dissolving tetrabutyl titanate in a citric acid ethanol solution, and stirring for 1-1.5 h; (b) adding tetraethoxysilane into the stirring liquid in the step (a); (c) heating the mixed solution in the step (b) to be not lower than 80 DEG C through a water bath, adding a metal salt aqueous solution of yttrium, and stirring until evaporation to obtain milk white wet gel; (d) putting the milk white wet gel in the step (c) into a drying oven, and heating for 2 hours under the condition that the temperature is not lower than 160 DEG C, so as to obtain puffed brown dry gel; (e) grinding the puffed brown xerogel in the step (d) to obtain precursor powder; and (f) putting the precursor powder in the step (e) into a muffle furnace, annealing at the temperature of not lower than 800 DEG C to obtain a white solid yttrium titanate doped material, and doping silicon ions in the yttrium titanate material to improve the wave-absorbing property of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new materials, and in particular to an yttrium titanate doped material, a preparation method and application thereof. Background Art

[0002] Electronic products have brought great convenience to people's daily lives, but they also bring a series of problems such as electromagnetic wave pollution. Electromagnetic wave radiation not only interferes with daily communications, but also worsens people's living environment. In addition, in the military field, electromagnetic wave absorbing materials can be used on the surface of aircraft to absorb electromagnetic waves emitted by radars, reducing the reconnaissance capability of the detection system. For the absorbing materials for the surface coating of aircraft, they must have the characteristics of thin coating, light weight, wide absorption frequency band and strong absorbing ability.

[0003] Yttrium titanate (chemical formula: Y2Ti2O7) is a strong dielectric compound with high dielectric constant and high temperature chemical stability, and has attracted more and more attention from researchers, see "Effects of calcium doping on yttriumtitanate for microwave absorbing applications", by Qinlong Wen; Wancheng Zhou; Yiding Wang; Fa Luo; Dongmei Zhu; Zhibin Huang; Yuchang Qing's journal article; and "Enhanced dielectric and microwave absorption properties of Y2Ti2O7 ceramicsby Sr doping", by Qinlong Wen; Wancheng Zhou; Hui Gao; Yingying Zhou; Fa Luo; Dongmei Zhu; Zhibin Huang; Yuchang Qing's journal article. Researchers usually dope yttrium titanate at the A site and use hot pressing to prepare Y 2-X Ca X Ti2O7 or Y 2-X Sr X Ti2O7, research Ca 2+ or Sr 2+ Replace Y 3+ The influence of defects, structure and physical properties of materials. In the X-band, when Ca 2+ When the doping reaches 10%, the reflection loss can reach -40.9dB (dB is the unit of decibel), and the effective absorption bandwidth is less than 1GHz; when Sr 2+When the doping reaches 7.5%, the reflection loss can reach -37.20dB and the effective absorption bandwidth is less than 1GHz.

[0004] In summary, the yttrium titanate material and the Ca-catalyzed yttrium titanate in the prior art 2+ or Sr 2+ The doped materials obtained by doping have poor wave absorbing properties and are not suitable for use as wave absorbing materials. Summary of the invention

[0005] In view of the above-mentioned deficiencies or defects in the prior art, the present invention provides a yttrium titanate doped material, a preparation method and an application thereof, and silicon ions are doped into the yttrium titanate material to improve the wave absorbing performance of the material.

[0006] In order to achieve the above object, the present invention provides a yttrium titanate doped material, which comprises yttrium titanate and doped silicon ions.

[0007] In some embodiments, the doping material is Y2Ti 2-x Si x O7, of which: 0 <X≤0.20。

[0008] The present invention also provides a preparation method for preparing the yttrium titanate doped material as described above, comprising the following preparation steps:

[0009] (a) dissolving tetrabutyl titanate in a citric acid ethanol solution and stirring for 1 to 1.5 hours to obtain a stirring solution;

[0010] (b) adding tetraethyl orthosilicate to the stirred solution obtained in step (a) to obtain a mixed solution;

[0011] (c) heating the mixed solution obtained in step (b) to not less than 80° C. in a water bath, adding an aqueous solution of yttrium metal salt to the mixed solution and stirring until the solution evaporates to obtain a milky white wet gel;

[0012] (d) placing the milky white wet gel obtained in step (c) into an oven and heating it at a temperature not lower than 160° C. for 2 h to obtain a puffed brown dry gel;

[0013] (e) grinding the expanded brown xerogel obtained in step (d) in a mortar to obtain a precursor powder;

[0014] (f) placing the precursor powder obtained in step (e) into a muffle furnace and annealing at a temperature not lower than 800° C. to obtain a white solid yttrium titanate doped material.

[0015] In some embodiments, in step (c), the aqueous solution of yttrium metal salt is yttrium nitrate hexahydrate.

[0016] In some embodiments, in step (c), the water bath heating temperature is 80°C to 90°C.

[0017] In some embodiments, in step (d), heating is performed at a temperature of 160°C to 180°C.

[0018] In some embodiments, the molar ratio of the metal salt of yttrium, the metal ion in tetrabutyl titanate, and citric acid is 1:1:(5-6).

[0019] In some embodiments, the molar ratio of the metal salt of yttrium, the metal ion in tetrabutyl titanate, and the citric acid is 1:1:5.

[0020] The present invention also provides an application of the yttrium titanate-doped material as described above, wherein the yttrium titanate-doped material is used as a wave absorbing material.

[0021] The yttrium titanate doped material using the above technical solution of the present invention has the following effects: silicon ions are doped into yttrium titanate to perform doping modification on the yttrium titanate and improve the wave absorbing performance of the material.

[0022] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The Y2Ti2O7 material in Comparative Example 1 and the Y2Ti2O7 material in Examples 1 to 3 are 2-X Si X X-ray diffraction pattern of O7-doped material;

[0024] Figure 2 The Y2Ti2O7 material in Comparative Example 1 and the Y2Ti2O7 material in Examples 1 to 3 are 2-X Si X Reflection loss diagram of O7 doped material;

[0025] Figure 3 It is Y2Ti of Example 1 1.95 Si 0.05 SEM images of O7-doped materials;

[0026] Figure 4 Y2Ti of Example 2 1.90 Si 0.10 SEM images of O7-doped materials;

[0027] Figure 5 It is Y2Ti of Example 3 1.85 Si 0.15 SEM images of O7-doped materials;

[0028] Figure 6This is a scanning electron microscope photograph of the Y2Ti2O7 material of comparative example 1. DETAILED DESCRIPTION

[0029] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0030] In the present invention, unless otherwise stated, the directional words such as "upper" and "lower" usually refer to the orientation in the assembled state. "Inside" and "outside" refer to the inside and outside relative to the outline of each component itself.

[0031] In a first aspect, the present invention discloses a yttrium titanate doped material, the doped material comprising yttrium titanate and doped silicon ions, the chemical formula of yttrium titanate is Y2Ti2O7, and the chemical formula of yttrium titanate doped with silicon ions is Y2Ti 2-x Si x O7. Yttrium titanate materials are modified by doping with silicon ions to improve the wave absorption performance of yttrium titanate doped materials.

[0032] In the present invention, preferably, the doping material comprises: <X≤0.20。

[0033] In a second aspect, the present invention discloses a method for preparing the above-mentioned yttrium titanate doped material, comprising the following steps:

[0034] (a) dissolving tetrabutyl titanate in a citric acid ethanol solution and stirring for 1 to 1.5 hours to obtain a stirring solution;

[0035] (b) adding tetraethyl orthosilicate to the stirred solution obtained in step (a) to obtain a mixed solution;

[0036] (c) heating the mixed solution obtained in step (b) to not less than 80° C. in a water bath, adding an aqueous solution of yttrium metal salt to the mixed solution and stirring until the solution evaporates to obtain a milky white wet gel;

[0037] (d) placing the milky white wet gel obtained in step (c) into an oven and heating it at a temperature not lower than 160° C. for 2 h to obtain a puffed brown dry gel;

[0038] (e) grinding the expanded brown xerogel obtained in step (d) in a mortar to obtain a precursor powder;

[0039] (f) placing the precursor powder obtained in step (e) into a muffle furnace and annealing at a temperature not lower than 800° C. to obtain a white solid yttrium titanate doped material.

[0040] At present, the commonly used method for preparing yttrium titanate doped materials is ball milling. Ball milling is a material preparation technology that disperses micron or submicron particles into an oil-based medium, such as kerosene, through long-term grinding to obtain a nano-level dispersion system. The basic principle of ball milling is to use the rotation or vibration of the ball mill to make the hard ball strongly impact, grind and stir the raw materials to obtain the desired nanomaterials. This method is simple to operate and low in cost, but the product purity is low and the particle size distribution is uneven. That is, the material prepared by the ball milling method has poor uniformity in properties and size, and has a discrete size distribution characteristic, which limits the further optimization of material properties. In addition, when using the ball milling method to prepare materials, the ball mill needs to work for more than 12 hours, and then sinter at 1500°C. The obtained pre-calcined powder is ball milled and dried again, and then hot-pressed and sintered at 1500°C. The entire preparation process consumes a lot of energy, the preparation process is cumbersome, and it is not suitable for large-scale industrial production.

[0041] In the present invention, the sol-gel method is adopted to evenly disperse the raw materials in the solvent, and a uniform mixing state at the molecular level can be quickly achieved. The prepared material has good chemical uniformity and is easier to achieve uniform doping. The powdered material synthesized by the preparation method disclosed in the present invention improves the purity of the material and improves the shape of the material, increases the specific surface area of ​​the material, and thus improves the wave absorption performance of the material. The sol-gel method uses a compound containing a highly chemically active component as a precursor, uniformly mixes the raw materials in the liquid phase, and performs hydrolysis and condensation chemical reactions to form a stable transparent sol system in the solution. The sol is aged and the particles are slowly polymerized to form a gel with a three-dimensional grid structure. The gel grid is filled with a solvent that has lost its fluidity to form a gel.

[0042] Optionally, in step (c), the aqueous solution of yttrium metal salt is yttrium nitrate hexahydrate. Yttrium metal nitrate is low in price and does not generate unnecessary products in the preparation method of the present invention.

[0043] Optionally, in step (c), the water bath heating temperature is 80°C to 90°C. While providing a sufficient water bath heating temperature, energy consumption can be reduced. In addition, the water bath heating temperature is 80°C and the stirring in step (a) is 1 to 1.5 hours, ensuring a sufficient stirring time and providing a sufficient water bath heating temperature, which can inhibit the hydrolysis of tetrabutyl titanate to form Ti(OH)4 (i.e., titanium hydroxide), so that no by-products are generated in the yttrium titanate doped material.

[0044] Optionally, in step (d), heating is performed at a temperature of 160° C. to 180° C. to reduce energy consumption while ensuring sufficient reaction.

[0045] Optionally, the molar ratio of the metal salt of yttrium, the metal ion in tetrabutyl titanate and the citric acid is 1:1:(5-6).

[0046] In the present invention, the molar ratio of yttrium metal salt, metal ions of tetrabutyl titanate and citric acid is 1:1:5. In the preparation process, too low a content of citric acid will cause tetrabutyl titanate to react with crystal water or water vapor in the air to generate titanium dioxide impurities, so citric acid can be appropriately excessive. That is, in other optional schemes, the molar ratio of yttrium metal salt, metal ions of tetrabutyl titanate and citric acid can also be 1:1:5.5 or 1:1:6.

[0047] Compared with the traditional solid phase method, the yttrium titanate doped material preparation method of the present invention has low energy consumption, and the prepared yttrium titanate material has the advantages of porous structure and large specific surface area. The porous structure can make the electromagnetic wave reflect multiple times after entering the material to further lose the electromagnetic wave, so as to enhance the material interface polarization and thus enhance the dielectric loss. The preparation process is simple and the production cost is low, which is suitable for large-scale production.

[0048] In a third aspect, the present invention also discloses a method of using yttrium titanate doped material as a radar absorbing material. Specifically, the yttrium titanate doped material can be used as a radar absorbing coating on aircraft and electronic products.

[0049] Embodiment 1:

[0050] Preparation of Yttrium Titanate Doped Material Y2Ti 2-X Si X O7 (X = 0.05).

[0051] (1) According to the material to be prepared, Y 3+ 、Ti 4+ and Si 4+ The molar ratio of Yttrium nitrate hexahydrate with a purity of 99.9% was 3.8301 g, tetrabutyl titanate was 3.3184 g, and ethyl orthosilicate was 0.0520 g. 3+ 9.6065 g of citric acid with a purity of 99% was weighed in a molar ratio of 1:5, yttrium nitrate hexahydrate was dissolved in 50 ml of deionized water to form a solution, and citric acid and 60 ml of anhydrous ethanol were mixed to obtain a citric acid ethanol solution.

[0052] (2) Dissolve tetrabutyl titanate in citric acid ethanol solution and stir for 1 to 1.5 hours to obtain a stirring liquid.

[0053] (3) Add tetraethyl orthosilicate to the stirring liquid to obtain a mixed solution.

[0054] (4) The mixed solution was heated to 80° C. in a water bath and maintained at 80° C., and yttrium nitrate hexahydrate solution was added to the mixed solution and stirred at a stirring speed of 200 r / min until the solution evaporated to obtain a milky white wet gel.

[0055] (5) The obtained milky white wet gel was placed in a forced air drying oven and heated at 160° C. for 2 h to obtain a puffed brown dry gel.

[0056] (6) The expanded brown dry gel is placed in a mortar and ground to obtain a precursor powder.

[0057] (7) The precursor powder was placed in a corundum crucible and placed in a muffle furnace. It was annealed at 800 °C for 2 h at a heating rate of 2 °C / min to obtain a white solid Y2Ti 1.95 Si 0.05 O7 powder.

[0058] Embodiment 2:

[0059] Preparation of Yttrium Titanate Doped Material Y2Ti 2-X Si X O7 (X = 0.10).

[0060] (1) According to the material to be prepared, Y 3+ 、Ti 4+ and Si 4+ The molar ratio of yttrium nitrate hexahydrate with a purity of 99.9% was 3.8301 g, tetrabutyl titanate was 3.2333 g, and ethyl orthosilicate was 0.1041 g. Then, according to Y 3+ 9.6065 g of citric acid with a purity of 99% was weighed in a molar ratio of 1:5, yttrium nitrate hexahydrate was dissolved in 50 ml of deionized water to form a solution, and citric acid and 60 ml of anhydrous ethanol were mixed to obtain a citric acid ethanol solution.

[0061] (2) Dissolve tetrabutyl titanate in citric acid ethanol solution and stir for 1 to 1.5 hours to obtain a stirring liquid.

[0062] (3) Add tetraethyl orthosilicate to the stirring liquid to obtain a mixed solution.

[0063] (4) The mixed solution was heated to 80° C. in a water bath and maintained at 80° C., and yttrium nitrate hexahydrate solution was added to the mixed solution and stirred at a stirring speed of 200 r / min until the solution evaporated to obtain a milky white wet gel.

[0064] (5) The obtained milky white wet gel was placed in a forced air drying oven and heated at 160° C. for 2 h to obtain a puffed brown dry gel.

[0065] (6) The expanded brown dry gel is placed in a mortar and ground to obtain a precursor powder.

[0066] (7) The precursor powder was placed in a corundum crucible and placed in a muffle furnace. It was annealed at 800 °C for 2 h at a heating rate of 2 °C / min to obtain a white solid Y2Ti 1.90 Si 0.10 O7 powder.

[0067] Embodiment 3:

[0068] Preparation of Yttrium Titanate Doped Material Y2Ti 2-X Si X O7 (X = 0.15).

[0069] (1) According to the material to be prepared, Y 3+ 、Ti 4+ and Si 4+ The molar ratio of Yttrium nitrate hexahydrate with a purity of 99.9% was 3.8301 g, tetrabutyl titanate was 3.1482 g, and ethyl orthosilicate was 0.1562 g. 3+ 9.6065 g of citric acid with a purity of 99% was weighed in a molar ratio of 1:5, yttrium nitrate hexahydrate was dissolved in 50 ml of deionized water to form a solution, and citric acid and 60 ml of anhydrous ethanol were mixed to obtain a citric acid ethanol solution.

[0070] (2) Dissolve tetrabutyl titanate in citric acid ethanol solution and stir for 1 to 1.5 hours to obtain a stirring liquid.

[0071] (3) Add tetraethyl orthosilicate to the stirring liquid to obtain a mixed solution.

[0072] (4) The mixed solution was heated to 80° C. in a water bath and maintained at 80° C., and yttrium nitrate hexahydrate solution was added to the mixed solution and stirred at a stirring speed of 200 r / min until the solution evaporated to obtain a milky white wet gel.

[0073] (5) The obtained milky white wet gel was placed in a forced air drying oven and heated at 160° C. for 2 h to obtain a puffed brown dry gel.

[0074] (6) The expanded brown dry gel is placed in a mortar and ground to obtain a precursor powder.

[0075] (7) The precursor powder was placed in a corundum crucible and placed in a muffle furnace. It was annealed at 800 °C for 2 h at a heating rate of 2 °C / min to obtain a white solid Y2Ti 1.85 Si 0.15 O7 powder.

[0076] Comparative Example 1:

[0077] Preparation of yttrium titanate material Y2Ti2O7, also known as Y2Ti 2-XSi X O7 (X = 0.00).

[0078] (1) According to the material to be prepared, Y 3+ and Ti 4+ The molar ratio of Yttrium nitrate hexahydrate with a purity of 99.9% was weighed 3.8301 g, tetrabutyl titanate was weighed 3.4035 g, and then according to Y 3+ 9.6065 g of citric acid with a purity of 99% was weighed in a molar ratio of 1:5, yttrium nitrate hexahydrate was dissolved in 50 ml of deionized water to form a solution, and citric acid and 60 ml of anhydrous ethanol were mixed to obtain a citric acid ethanol solution.

[0079] (2) Dissolve tetrabutyl titanate in citric acid ethanol solution and stir for 1 to 1.5 hours to obtain a stirring liquid.

[0080] (3) The stirred liquid was heated to 80° C. in a water bath and maintained at 80° C., and yttrium nitrate hexahydrate solution was added to the stirred liquid and stirred at a stirring speed of 200 r / min until the solution evaporated to obtain a milky white wet gel.

[0081] (4) The obtained milky white wet gel was placed in a forced air drying oven and heated at 160° C. for 2 h to obtain a puffed brown dry gel.

[0082] (5) The expanded brown dry gel is put into a mortar and ground to obtain a precursor powder.

[0083] (6) The precursor powder was placed in a corundum crucible and placed in a muffle furnace. It was annealed at 800 °C for 2 h at a heating rate of 2 °C / min to obtain a white solid Y2Ti2O7 powder.

[0084] Comparative Example 2:

[0085] According to the prior art, Ca doped in yttrium titanate material is prepared 2+ Up to 10% of the resulting material.

[0086] Comparative Example 3:

[0087] According to the prior art, Sr doped in yttrium titanate material is prepared. 2+ Reach 7.5% of the resulting material.

[0088] The performance of the materials obtained in each embodiment and comparative example was tested, and the test results are shown in Table 1.

[0089] Table 1

[0090] Maximum reflection loss / dB Effective absorption bandwidth / GHz Example 1 -38.04 1.88 Example 2 -54.05 2.92 Example 3 -36.58 2.92 Comparative Example 1 -14.49 1.56 Comparative Example 2 -40.90 <1 Comparative Example 3 -37.20 <1

[0091] In the attached Figure 1In the figure, the horizontal axis represents the X-ray diffraction angle, and the vertical axis represents the diffraction intensity of the material. The YT curve represents Y2Ti2O7, or Y2Ti 2-X Si X X-ray diffraction intensity curve of O7 (X = 0.00) material; 0.05Si curve represents Y2Ti 2- X Si X X-ray diffraction intensity curve of O7 (X = 0.05) material; 0.10Si curve represents Y2Ti 2-X Si X X-ray diffraction intensity curve of O7 (X = 0.10) material; 0.15Si curve represents Y2Ti 2-X Si X X-ray diffraction intensity curve of O7 (X=0.15) material.

[0092] In the attached Figure 2 In the reflection loss graph, the horizontal axis represents the frequency range of the material performance test, and the vertical axis represents the reflection loss of the material's wave absorption performance. The smaller the reflection loss, the more electromagnetic waves the material absorbs, and the better the wave absorption performance. In the present invention, it refers to the ability of the material to effectively absorb electromagnetic waves in the frequency range of 2 to 18 GHz. When the reflection loss reaches below -10 dB, absorbing 90% of the electromagnetic waves is the effective absorption of electromagnetic waves. It should be noted that the effective absorption bandwidth refers to the maximum frequency width of the continuous curve when the reflection loss curve of the material reaches below -10 dB, and is not the sum of all frequency widths when the reflection loss curve reaches below -10 dB.

[0093] The wave absorption performance of the materials in the examples and comparative examples should be judged by comprehensively considering the two indicators of reflection loss and effective absorption bandwidth. 2-X Si X O7 (X = 0.10) material, the maximum reflection loss is -54.05dB, and the effective absorption bandwidth is 2.92GHz. Compared with other embodiments and comparative examples, the yttrium titanate composite material in Example 2 has the best comprehensive wave absorption performance.

[0094] Scanning electron microscope is mainly used to observe the surface morphology of materials and whether the prepared materials are porous structures. The quality of porous structures needs to be evaluated by combining two indicators: pore size and pore density. Figure 3 To Attachment Figure 6 , Y2Ti in Example 2 provided by the present invention 2-X Si X The porous structure of the O7 (X=0.10) material is the best compared with other embodiments and comparative examples. The porous structure is conducive to enhancing the dielectric loss of the material, thereby improving the wave absorbing performance of the material.

[0095] The reflection loss curves and scanning electron microscope photos of Comparative Example 2 and Comparative Example 3 can be found in the journal articles “Effects of calcium doping on yttrium titanate for microwave absorbing applications” and “Enhanced dielectric and microwave absorption properties of Y2Ti2O7 ceramics by Sr doping”.

[0096] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0097] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0098] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A yttrium titanate doped material, characterized in that: The doping material includes yttrium titanate and doped silicon ions.

2. The yttrium titanate doped material according to claim 1, characterized in that: The doping material is Y2Ti 2-x Si x O7, of which: 0 <X≤0.20。 3. A preparation method for preparing the yttrium titanate doped material according to claim 1 or 2, characterized in that: The method comprises the following preparation steps: (a) dissolving tetrabutyl titanate in a citric acid ethanol solution and stirring for 1 to 1.5 hours to obtain a stirring solution; (b) adding tetraethyl orthosilicate to the stirred solution obtained in step (a) to obtain a mixed solution; (c) heating the mixed solution obtained in step (b) to not less than 80° C. in a water bath, adding an aqueous solution of yttrium metal salt to the mixed solution and stirring until the solution evaporates to obtain a milky white wet gel; (d) placing the milky white wet gel obtained in step (c) into an oven and heating it at a temperature not lower than 160° C. for 2 h to obtain a puffed brown dry gel; (e) grinding the expanded brown xerogel obtained in step (d) in a mortar to obtain a precursor powder; (f) placing the precursor powder obtained in step (e) into a muffle furnace and annealing at a temperature not lower than 800° C. to obtain a white solid yttrium titanate doped material.

4. The preparation method according to claim 3, characterized in that: In step (c), the aqueous solution of yttrium metal salt is yttrium nitrate hexahydrate.

5. The preparation method according to claim 3, characterized in that: In step (c), the water bath heating temperature is 80°C to 90°C.

6. The preparation method according to claim 3, characterized in that: In step (d), heating is performed at a temperature of 160°C to 180°C.

7. The preparation method according to claim 3, characterized in that: The molar ratio of the metal salt of yttrium, the metal ion in tetrabutyl titanate and the citric acid is 1:1:(5-6).

8. The preparation method according to claim 7, characterized in that: The molar ratio of the metal salt of yttrium, the metal ion in tetrabutyl titanate and the citric acid is 1:1:

5.

9. An application of the yttrium titanate doped material as claimed in claim 1 or 2, characterized in that: Yttrium titanate doped material is used as a microwave absorbing material.