Solid-liquid phase change thermal interface material and preparation method thereof
Through the design of solid-liquid phase heat-changing interface materials, combined with paraffin, filled powder and alumina fibers, the problem of insufficient thermal conductivity of silicone rubber heat dissipation gaskets is solved, and high thermal conductivity and easy processing is achieved. It is suitable for new electronic products. , has promoted the promotion and application of electronic products.
Patent Information
- Application Number
- CN202411175025.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing silicone rubber heat dissipation gaskets are difficult to exert sufficient thermal conductivity in new high-performance microprocessors, graphics processors, chips and other electronic products, which limits the promotion and application of electronic products.
Using solid-liquid phase change thermal interface material, a combination of paraffin, filled powder, alumina fibers and additives is used to form a thermal interface material with temperature-dependent solid-liquid phase change characteristics, combined with vacuum impregnation and coating processes to improve thermal conductivity And enhance processing ease.
It overcomes the problem of insufficient thermal conductivity of silicone rubber heat dissipation gaskets, achieves higher thermal conductivity and easy processing, is suitable for new electronic products, significantly improves the thermal conductivity coefficient, and meets the needs of high-performance electronic products.
Smart Images

Figure BDA0005010491050000061 
Figure BDA0005010491050000081 
Figure BDA0005010491050000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of thermal conductive materials, and more specifically, to a solid-liquid phase change thermal interface material and a preparation method thereof. Background Art
[0002] At present, the application of electronic devices has penetrated into all walks of life. In some special types of electronic devices, there are power-consuming components that generate a lot of heat. When these power-consuming components are working, the accumulation of heat will affect the overall operation of the electronic equipment, so a heat sink is often required. In order to improve the heat dissipation efficiency of the heat sink, it is also necessary to set a material with good thermal conductivity as a filler between the power-consuming components and the heat sink. This type of material is usually called a thermal interface material.
[0003] In the related art, there is a thermal interface material made of silicone rubber, also called silicone rubber heat sink. The thermal conductivity of this thermal interface material is usually between 5-6W / m·K, and the thickness is 10-150mil. The advantages are that it has a certain degree of flexibility, can be deformed, and can be reused, which is convenient to use.
[0004] Regarding the above-mentioned related technologies, the inventors believe that the advantages of the silicone rubber heat dissipation gaskets in the related technologies are mainly reflected in their ease of use. However, with the rapid development of electronic products, in the application of new high-performance microprocessors, graphics processors, chips and other important parts of electronic products, this thermal interface material is difficult to exert sufficient thermal conductivity, which has hindered the promotion and application of electronic products. Summary of the invention
[0005] In the related art, silicone rubber heat sink gaskets are difficult to exert sufficient thermal conductivity in applications such as new high-performance microprocessors, graphics processors, chips and other important parts of electronic products. In order to improve this defect, the present application provides a solid-liquid phase change thermal interface material and a preparation method thereof.
[0006] In a first aspect, the present application provides a solid-liquid phase change thermal interface material, which adopts the following technical solution: A solid-liquid phase change thermal interface material, comprising the following components in parts by weight: 10-12 parts of paraffin, 90-95 parts of filling powder, 4-8 parts of alumina fiber, and 0.5-1.0 parts of an auxiliary agent. The filling powder comprises a first powder component and a second powder component. The first powder component comprises aluminum nitride powder, and the second powder component comprises one of aluminum oxide powder, zinc oxide powder, and nano aluminum powder. The weight of the first powder component accounts for 20-52% of the total weight of the filling powder.
[0007] By adopting the above technical scheme, the present application uses filling powder as the main component, and obtains a new thermal interface material by mixing paraffin, filling powder, alumina fiber and additives. At room temperature, this thermal interface material is easy to cut, and after being heated, the paraffin will melt, so that the thermal interface material is converted from solid to paste. In this state, this thermal interface material has good processability and can be more fully bonded to the substrate. At the same time, the addition of filling powder, alumina fiber and other components enables the thermal interface material of the present application to exert thermal conductivity better than that of silicone rubber gaskets. The thermal interface material of the present application has the characteristics of solid-liquid phase change according to temperature, and has easy processability and good thermal conductivity. It can also be used in combination with silicone rubber heat dissipation gaskets, overcoming the defect that the thermal conductivity of silicone rubber heat dissipation gaskets is difficult to meet actual needs. It can exert sufficient thermal conductivity in the application of important parts of new high-performance microprocessors, graphics processors, chips and other electronic products, which is conducive to the promotion and application of new electronic products.
[0008] Preferably, the first powder component comprises modified aluminum nitride powder, the weight ratio of the modified aluminum nitride powder to the aluminum nitride powder is 1:(1.2-1.9), and the modified aluminum nitride powder is prepared according to the following method: (1) mixing aluminum nitride powder, oleic acid, and anhydrous ethanol to obtain a mixed solution with a mass fraction of 7-9% of aluminum nitride powder, and allowing the mixed solution to stand for use; the amount of oleic acid used is 0.5-2.5% of the weight of the aluminum nitride powder; (2) After the mixed solution is allowed to stand for 2-3 hours, polyethylene glycol is added to the mixed solution, and the mixed solution is heated in a water bath at 50-60° C. for 3-6 hours, and then filtered and the filter residue is washed with an organic solvent, and the filter residue is dried for later use to obtain modified aluminum nitride powder.
[0009] By adopting the above technical solution, the present application uses oleic acid to treat aluminum nitride powder, so that oleic acid is adsorbed on the surface of aluminum nitride powder to obtain modified aluminum nitride powder. The long-chain hydrocarbon group of oleic acid has good compatibility with paraffin, so the modified aluminum nitride powder can be in more sufficient contact with paraffin, reducing the interfacial thermal resistance between the filling powder and paraffin, which helps to improve the thermal conductivity of the thermal interface material.
[0010] Preferably, the amount of oleic acid used is 1.7-2.5% of the weight of the aluminum nitride powder.
[0011] By adopting the above technical solution, the present application optimizes the dosage of oleic acid, which helps to improve the thermal conductivity of the thermal interface material.
[0012] Preferably, the weight ratio of the modified aluminum nitride powder to the aluminum nitride powder is 1:(1.2-1.5).
[0013] By adopting the above technical solution, the present application optimizes the ratio of modified aluminum nitride powder to aluminum nitride powder, which helps to improve the thermal conductivity of the thermal interface material.
[0014] Preferably, the weight of the first powder component accounts for 30-52% of the total weight of the filling powder.
[0015] By adopting the above technical solution, the present application optimizes the proportion of the first powder component in the filling powder, which helps to improve the thermal conductivity of the thermal interface material.
[0016] Preferably, the filling powder D 100 Particle size is 10-30μm, D 50 The particle size is 3-10μm.
[0017] By adopting the above technical solution, the present application optimizes the particle size distribution parameters of the filling powder. The filling powder prepared according to the above particle size distribution parameters can be mixed with the paraffin melt to form a paste, and has good processability.
[0018] Preferably, the filling powder D 100 Particle size is 10-18μm, D 50 The particle size is 3-6μm.
[0019] By adopting the above technical solution, the present application preferably selects D of the filling powder. 100 Particle size, on the basis of the aforementioned preferred embodiment, removes particles with relatively large particle sizes, reduces the impact of large particle sizes on the grading of the filling powder, increases the proportion of small particle sizes, and allows the particles of the filling powder to be more fully filled, which helps to improve the thermal conductivity of the thermal interface material.
[0020] Preferably, the alumina fiber is formed by mixing a first alumina fiber and a second alumina fiber in a weight ratio of 1:(1.3-2.1), the first alumina fiber is an alumina fiber prepared by a melt spinning method, and the second alumina fiber is prepared according to the following method: (1) dissolving urea and sodium hydroxide in water to obtain a modification solution with a mass fraction of 7% sodium hydroxide and a mass fraction of 12% urea, soaking sisal fiber in the modification solution at a bath ratio of 1:20 at -12°C for 30 minutes, then taking out the sisal fiber and drying it to obtain a fiber template; (2) Soaking the fiber template in an aluminum chloride solution for 60-90 minutes, then removing the fiber template, calcining it at 1200-1280° C. for 120-130 minutes, and then crushing it to obtain a second alumina fiber.
[0021] By adopting the above technical solution, the present application uses a modified liquid to dissolve a part of the cellulose in the sisal fiber on the basis of the sisal fiber to obtain a fiber template, and then uses the fiber template as a matrix to convert aluminum chloride into aluminum oxide by immersing it in an aluminum chloride solution and then calcining it, and the undissolved part of the fiber template is removed during the calcination process, so that the obtained fiber has a certain porosity and can be in contact with paraffin for heat transfer more fully. Therefore, by preparing aluminum oxide fiber according to the above method, the thermal conductivity of the thermal interface material can be more fully improved.
[0022] Preferably, the alumina fiber is formed by mixing a first alumina fiber and a second alumina fiber in a weight ratio of 1:(1.7-2.1).
[0023] By adopting the above technical solution, the present application optimizes the ratio of the first alumina fiber and the second alumina fiber, which helps to fully improve the thermal conductivity of the thermal interface material.
[0024] In a second aspect, the present application provides a method for preparing a solid-liquid phase change thermal interface material, which adopts the following technical solution.
[0025] A method for preparing a solid-liquid phase change thermal interface material comprises the following steps: (1) mixing alumina fiber, filler powder and additives, and then mixing and stirring with molten paraffin to obtain a premix; (2) The premix is vacuum impregnated for 5-7 minutes, and then coated onto the surface of a sheet material serving as a substrate, and then cooled to obtain a solid-liquid phase change thermal interface material.
[0026] By adopting the above technical solution, the present application first prepares a premix, then vacuum impregnates the premix, and then performs coating and cooling molding to obtain a solid-liquid phase change thermal interface material.
[0027] In summary, this application has the following beneficial effects: 1. The thermal interface material of the present application has the property of undergoing solid-liquid phase change according to temperature, and can be converted into a paste after being heated. It has the same ease of processing as silicone rubber heat sink gaskets, and at the same time can exert good thermal conductivity, overcoming the defect that the thermal conductivity of silicone rubber heat sink gaskets is difficult to meet actual needs, and is conducive to the promotion and application of new electronic products.
[0028] 2. In this application, the particle size distribution of the filling powder is optimized by reducing D 100 Particle size and D 50 The particle size improves the particle gradation of the filling powder, allowing the particles to be filled more fully, which helps to improve the thermal conductivity of the thermal interface material. DETAILED DESCRIPTION
[0029] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.
[0030] Preparation example of modified aluminum nitride powder The following is an explanation using Preparation Example 1.
[0031] Preparation Example 1 In this preparation example, the modified aluminum nitride powder was prepared according to the following method: (1) Aluminum nitride powder, oleic acid, and anhydrous ethanol are mixed and stirred to obtain a mixed solution having an aluminum nitride powder mass fraction of 7% (referred to as aluminum nitride content in Table 1), and the mixed solution is allowed to stand for use; the amount of oleic acid used is 0.5% of the weight of the aluminum nitride powder; (2) After the mixed solution was allowed to stand for 2 h (referred to as the standing time in Table 1), polyethylene glycol (PEG-200) was added to the mixed solution, and the mixed solution was heated in a water bath at 50° C. (referred to as the water bath temperature in Table 1) for 3 h (referred to as the water bath time in Table 1), and then filtered and the filter residue was washed with an organic solvent, and the filter residue was dried for use to obtain modified aluminum nitride powder.
[0032] As shown in Table 1, the differences between Preparation Examples 1-5 are the aluminum nitride content in the mixed solution and some production and processing parameters.
[0033] Table 1 Aluminum nitride content and some production and processing parameters sample Aluminum nitride content / % Standing time / h Water bath temperature / ℃ Water bath time / h Preparation Example 1 7 2 50 3 Preparation Example 2 7.5 2.5 52 4 Preparation Example 3 8 2.5 55 4 Preparation Example 4 8.5 3 58 5 Preparation Example 5 9 3 60 6 Preparation Example 5-9 As shown in Table 2, the difference between Preparation Examples 5-9 is that the percentage of oleic acid used in the weight of aluminum nitride (abbreviated as oleic acid percentage in Table 2) is different.
[0034] Table 2 Oleic acid ratio sample Oleic acid percentage / % Preparation Example 5 0.5 Preparation Example 6 1.0 Preparation Example 7 1.7 Preparation Example 8 2.1 Preparation Example 9 2.5 Preparation Example of the Second Alumina Fiber The following is an explanation using Preparation Example 10 as an example.
[0035] Preparation Example 10 In this preparation example, the sisal fibers used had an average diameter of 120 μm.
[0036] In this preparation example, the second alumina fiber is prepared according to the following method: (1) dissolving urea and sodium hydroxide in water to obtain a modification solution with a mass fraction of 7% sodium hydroxide and a mass fraction of 12% urea, soaking sisal fiber in the modification solution at a bath ratio of 1:20 at -12°C for 30 minutes, then taking out the sisal fiber and drying it to obtain a fiber template; (2) The fiber template was immersed in an aluminum chloride solution with a mass concentration of 20% at a bath ratio of 1:10 for 60 minutes (referred to as the immersion time in Table 3), and then the fiber template was removed and calcined at 1200°C (referred to as the calcination temperature in Table 3) for 120 minutes (referred to as the calcination time in Table 3). After crushing, a second alumina fiber with an average length of 1.5 mm was obtained.
[0037] As shown in Table 3, the difference between Preparation Examples 10-14 is that the production and processing parameters of the second alumina fiber are different.
[0038] Table 3 Production and processing parameters of the second alumina fiber sample Soaking time / min Calcination temperature / ℃ Calcination time / min Preparation Example 10 60 1200 120 Preparation Example 11 70 1220 122 Preparation Example 12 75 1240 125 Preparation Example 13 80 1260 128 Preparation Example 14 90 1280 130 Example
[0039] Examples 1-5 The following description is given by taking Example 1 as an example.
[0040] Example 1 This embodiment provides a solid-liquid phase change thermal interface material, which is composed of the following components: 10kg paraffin, 90kg filling powder, 4kg alumina fiber, and 0.5kg additive. The paraffin is commercial paraffin (pure paraffin, PW, melting point 58°C), the filling powder includes a first powder component and a second powder component, the first powder component is aluminum nitride powder, the second powder component is alumina powder, the weight of the first powder component accounts for 20% of the total weight of the filling powder, and the rest is supplemented by the second powder component to 100%; D of the filling powder 100 The particle size is 30 μm, D 50 The particle size is 10 μm; the alumina fiber is a commercially available product obtained by melt spinning, and the average diameter of the alumina fiber is 120 μm and the average length is 1.5 mm; the auxiliary agent is a mixture of a silicone rubber delay agent (YL-O4) and a silicone rubber catalyst (dibutyltin diacetate) in a weight ratio of 3:1.
[0041] In this embodiment, the sheet material used as the substrate is a silicone rubber heat dissipation pad with a thickness of 70 mil and a thermal conductivity of 5.89 W / m·K.
[0042] In this embodiment, the solid-liquid phase change thermal interface material is prepared according to the following steps: (1) Alumina fiber, filler powder and additives are mixed, and then mixed with molten paraffin and stirred at a rate of 200 r / min to obtain a premix; (2) The premix is vacuum impregnated for 5 minutes (referred to as the impregnation time in Table 4) and then coated onto the surface of a sheet material serving as a substrate. After cooling, a solid-liquid phase change thermal interface material having a thickness of 50 mil is obtained.
[0043] In Example 5, the dosage of the nano aluminum powder is 5% of the weight of the zinc oxide powder, and the particle size of the nano aluminum powder is 50 nm.
[0044] As shown in Table 4, the differences between Examples 1-5 mainly lie in the different raw material ratios and production and processing parameters of the solid-liquid phase change thermal interface materials.
[0045] Table 4 Different raw material ratios and production and processing parameters of solid-liquid phase change thermal interface materials Example 6 The difference between this embodiment and embodiment 5 is that the first powder component is formed by mixing the modified aluminum nitride powder of preparation example 1 and the aluminum nitride powder used in embodiment 1 in a weight ratio of 1:1.9.
[0046] As shown in Table 5, the difference between Examples 6-14 is that the preparation examples of the modified aluminum nitride powder are different.
[0047] Table 5 Preparation example of modified aluminum nitride powder sample Preparation Example sample Preparation Example Example 6 Preparation Example 1 Embodiment 11 Preparation Example 6 Example 7 Preparation Example 2 Example 12 Preparation Example 7 Example 8 Preparation Example 3 Embodiment 13 Preparation Example 8 Example 9 Preparation Example 4 Embodiment 14 Preparation Example 9 Example 10 Preparation Example 5 / / Examples 14-18 As shown in Table 6, the difference between Examples 14-18 is that the weight ratio of the modified aluminum nitride powder to the aluminum nitride powder (hereinafter referred to as the aluminum nitride ratio) is different.
[0048] Table 6 Aluminum nitride ratio sample Aluminum Nitride Ratio Embodiment 14 1:1.9 Embodiment 15 1:1.7 Example 16 1:1.5 Embodiment 17 1:1.4 Embodiment 18 1:1.2 Examples 18-22 The difference between this embodiment and embodiment 7 is that the percentage of the weight of the first powder component to the total weight of the filling powder (hereinafter referred to as the first powder component percentage) is different.
[0049] Table 7 sample The first powder component ratio / % Embodiment 18 20 Embodiment 19 25 Embodiment 20 30 Embodiment 21 41 Embodiment 22 52 Examples 22-26 As shown in Table 8, the difference between Examples 22-26 is that the D 100 Particle size and D 50 Different particle sizes.
[0050] Table 8 sample <![CDATA[D 100 Particle size / μm]]> <![CDATA[D 50 Particle size / μm]]> Embodiment 22 30 10 Embodiment 23 22 8 Embodiment 24 18 6 Embodiment 25 14 5 Embodiment 26 10 3 Embodiment 27 The difference between this embodiment and Embodiment 26 is that the alumina fiber is formed by mixing a first alumina fiber and a second alumina fiber in a weight ratio of 1:1.3; the first alumina fiber is the alumina fiber used in Embodiment 26, and the second alumina fiber is prepared according to the method of Preparation Example 10.
[0051] As shown in Table 9, the difference between Examples 27-31 is that the preparation examples of alumina fibers are different.
[0052] Table 9 Preparation example of alumina fiber sample Preparation Example Embodiment 27 Preparation Example 10 Embodiment 28 Preparation Example 11 Embodiment 29 Preparation Example 12 Embodiment 30 Preparation Example 13 Embodiment 31 Preparation Example 14 Examples 31-35 As shown in Table 10, the difference between Examples 31-35 is that the weight ratio of the first alumina fiber and the second alumina (referred to as fiber ratio in Table 10) is different.
[0053] Table 10 Fiber Ratio Comparative Example Comparative Example 1 This comparative example provides a thermal interface material, specifically a commercially available silicone rubber heat dissipation pad with a thickness of 120 mil and a thermal conductivity of 5.89 W / m·K.
[0054] Comparative Example 2 The difference between this comparative example and Example 1 is that the filling powder consists only of alumina powder.
[0055] Performance testing methods According to the principle of steady-state heat flow method, a solid thermal conductivity tester (TC 3000, Xiaxi Company, Xi'an) was used to detect the thermal conductivity of the thermal interface materials of each embodiment and comparative example along the thickness direction, and the thermal conductivity of comparative example 1 was used as a benchmark to calculate the ratio between the thermal conductivity of each embodiment and comparative example and the thermal conductivity of comparative example 1. The ratio was recorded as the relative thermal conductivity and expressed as a percentage. The results are shown in Table 11.
[0056] Table 11 Relative thermal conductivity It can be seen from Examples 1-5 and Comparative Example 1 and Table 11 that the relative thermal conductivity coefficients measured in Examples 1-5 are all higher than those in Comparative Example 1, indicating that after the solid-liquid phase change thermal interface material of the present application is compounded with the silicone rubber heat dissipation gasket, the obtained composite thermal interface material has better thermal conductivity than the silicone rubber heat dissipation gasket of the same thickness, overcoming the defect that the thermal conductivity of the silicone rubber heat dissipation gasket is difficult to meet actual needs, which is conducive to the promotion and application of new electronic products.
[0057] Combining Example 1 and Comparative Example 2 and Table 11, it can be seen that the relative thermal conductivity measured in Example 1 is higher than that in Comparative Example 1, indicating that the addition of aluminum nitride plays a key role in improving the thermal conductivity of the thermal interface material.
[0058] It can be seen from Example 5 and Examples 6-10 and Table 11 that by replacing a portion of the aluminum nitride powder with modified aluminum nitride powder, the thermal conductivity of the solid-liquid phase change thermal interface material can be improved to a certain extent.
[0059] It can be seen from Examples 10-14 and Table 11 that in the method for preparing modified aluminum nitride powder, when the amount of oleic acid is 1.7-2.5% of the weight of the aluminum nitride powder, the thermal conductivity of the solid-liquid phase change thermal interface material is relatively good.
[0060] It can be seen from Examples 14-18 and Table 11 that when the weight ratio of the modified aluminum nitride powder to the aluminum nitride powder is 1:(1.2-1.5), the thermal conductivity of the solid-liquid phase change thermal interface material is relatively good.
[0061] It can be seen from Examples 18-22 and Table 11 that when the weight of the first powder component accounts for 30-52% of the total weight of the filling powder, the thermal conductivity of the solid-liquid phase change thermal interface material is relatively good.
[0062] Combining Examples 22-26 and Table 11, it can be seen that when the D of the filling powder 100 Particle size is 10-30μm, D 50 When the particle size is 3-10 μm, the thermal conductivity of the solid-liquid phase change thermal interface material is relatively good.
[0063] It can be seen from Example 26, Examples 27-31 and Table 11 that the addition of the second alumina fiber can improve the thermal conductivity of the solid-liquid phase change thermal interface material.
[0064] It can be seen from Examples 31-35 and Table 11 that when the alumina fiber is mixed with the first alumina fiber and the second alumina fiber in a weight ratio of 1:(1.7-2.1), the thermal conductivity of the solid-liquid phase change thermal interface material is relatively good.
[0065] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A solid-liquid phase change thermal interface material, characterized in that: The invention comprises the following components in parts by weight: 10-12 parts of paraffin, 90-95 parts of filling powder, 4-8 parts of alumina fiber, and 0.5-1.0 parts of additives. The filling powder comprises a first powder component and a second powder component. The first powder component comprises aluminum nitride powder, and the second powder component comprises one of alumina powder, zinc oxide powder, and nano aluminum powder. The weight of the first powder component accounts for 20-52% of the total weight of the filling powder.
2. The solid-liquid phase change thermal interface material according to claim 1, characterized in that: The first powder component includes modified aluminum nitride powder, the weight ratio of the modified aluminum nitride powder to the aluminum nitride powder is 1:(1.2-1.9), and the modified aluminum nitride powder is prepared according to the following method: (1) mixing aluminum nitride powder, oleic acid and anhydrous ethanol to obtain a mixed solution with a mass fraction of 7-9% of aluminum nitride powder, and allowing the mixed solution to stand for use; the amount of oleic acid used is 0.5-2.5% of the weight of the aluminum nitride powder; (2) After the mixed solution is allowed to stand for 2-3 hours, polyethylene glycol is added to the mixed solution, and the mixed solution is heated in a water bath at 50-60° C. for 3-6 hours. The mixed solution is then filtered and the filter residue is washed with an organic solvent. The filter residue is dried for later use to obtain modified aluminum nitride powder.
3. The solid-liquid phase change thermal interface material according to claim 2, characterized in that: The amount of oleic acid used is 1.7-2.5% of the weight of the aluminum nitride powder.
4. The solid-liquid phase change thermal interface material according to claim 3, characterized in that: The weight ratio of the modified aluminum nitride powder to the aluminum nitride powder is 1:(1.2-1.5).
5. The solid-liquid phase change thermal interface material according to claim 4, characterized in that: The weight of the first powder component accounts for 30-52% of the total weight of the filling powder.
6. The solid-liquid phase change thermal interface material according to claim 1, characterized in that: The filling powder D 100 Particle size is 10-30μm, D 50 The particle size is 3-10μm.
7. The solid-liquid phase change thermal interface material according to claim 6, characterized in that: The filling powder D 100 Particle size is 10-18μm, D 50 The particle size is 3-6μm.
8. The solid-liquid phase change thermal interface material according to claim 1, characterized in that: The alumina fiber is formed by mixing a first alumina fiber and a second alumina fiber in a weight ratio of 1:(1.3-2.1), wherein the first alumina fiber is an alumina fiber prepared by a melt spinning method, and the second alumina fiber is prepared by the following method: (1) Dissolving urea and sodium hydroxide in water to obtain a modification solution with a mass fraction of 7% sodium hydroxide and a mass fraction of 12% urea, soaking sisal fiber in the modification solution at a bath ratio of 1:20 at -12°C for 30 minutes, then taking out the sisal fiber and drying it to obtain a fiber template; (2) Soaking the fiber template in an aluminum chloride solution for 60-90 minutes, then removing the fiber template, calcining it at 1200-1280° C. for 120-130 minutes, and then crushing it to obtain a second alumina fiber.
9. The solid-liquid phase change thermal interface material according to claim 8, characterized in that: The alumina fiber is formed by mixing a first alumina fiber and a second alumina fiber in a weight ratio of 1:(1.7-2.1).
10. The method for preparing the solid-liquid phase change thermal interface material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Alumina fiber, filler powder and additives are mixed, and then mixed with molten paraffin and stirred to obtain a premix; (2) The premix is vacuum impregnated for 5-7 minutes and then coated onto the surface of a sheet material serving as a substrate. After cooling, a solid-liquid phase change thermal interface material is obtained.