Crop straw biomass chemical heat storage gel as well as preparation method and application thereof
By using crop straw biomass chemical heat storage gel, the problems of poor heating sustainability and high carbon emissions in solar heavy oil thermal production are solved, efficient heavy oil steam driving and carbon capture are achieved, and heavy oil thermal production is improved. Productivity and environmental friendliness.
Patent Information
- Application Number
- CN202411036012.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-12-03
AI Technical Summary
The existing solar heavy oil thermal production technology has problems such as poor heating sustainability, low energy efficiency and high carbon emissions, resulting in a decrease in heavy oil production and a decline in economic profits.
Using crop straw biomass chemical heat storage gel as a mixing agent, carbonate as chemical heat storage functional filler and carbon material as thermal conductivity agent, build a strong gel network through biopolymer gelling agents, and improve heat storage capacity and Carbon capture efficiency.
Effectively enhance the sustainability of solar heating, improve the steam recovery rate and energy efficiency of heavy oil, reduce carbon emissions, achieve all-weather heavy oil production, and absorb and fix a large amount of CO2 during the heat release process.
Smart Images

Figure CN119060698A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of petroleum extraction, and in particular to a crop straw biomass chemical heat storage gel and a preparation method and application thereof. Background Art
[0002] With the continuous growth of global demand for fossil energy and the depletion of traditional crude oil reservoirs, heavy oil resources are becoming increasingly important for industrial development. Steam injection recovery (mainly including steam throughput, steam drive and steam-assisted gravity drainage, etc.) is the current mainstream method of heavy oil recovery, which mainly relies on input heat to reduce the viscosity of heavy oil to improve its fluidity and recoverability. However, the above-mentioned steam-based thermal recovery method requires the combustion of a large amount of fossil energy (mainly natural gas) to generate sufficient high-temperature steam for oil recovery, resulting in high energy consumption. At the same time, combustion causes a large amount of greenhouse gas emissions, resulting in serious environmental problems, and significantly increases the policy resistance and economic costs (carbon tax) of heavy oil recovery.
[0003] In order to effectively reduce the energy consumption of heavy oil thermal recovery, researchers have developed a series of solar heating heavy oil thermal recovery systems, using solar collectors (including linear Fresnel reflectors, parabolic troughs, solar towers and parabolic reflectors) to generate high-temperature superheated steam (150℃~1000℃) to replace or partially replace fossil fuel combustion. With the application of the above-mentioned solar steam generators, the fossil fuel consumption in the heavy oil thermal recovery process has been significantly reduced, with a saving of 25%~80%. However, the intermittent and diurnal nature of solar energy (weather and sunset have an important impact on solar heating) makes it impossible to achieve continuous steam supply to complete 24×7 all-weather crude oil industrial production, resulting in reduced heavy oil production and reduced economic profits. At the same time, the high heterogeneity of heavy oil reservoirs and the high density difference between heavy oil and steam cause strong steam crossflow and gravity overburden, resulting in low energy efficiency of solar heavy oil thermal recovery process. In order to effectively improve the production efficiency of solar heavy oil thermal recovery, oil fields currently extend the operation time of solar steam flooding mainly through the following two methods: 1) solar-powered heavy oil thermal recovery during the day and steam flooding heated by natural gas at night. This method can significantly make up for the insufficient heating caused by the intermittent solar radiation, effectively improve the continuity of heating and thermal recovery efficiency. However, the large amount of natural gas consumption reduces the energy-saving and emission-reduction effect of solar heavy oil thermal recovery. 2) Expand the solar field area and add inorganic salt heat storage materials to the collector. This method mainly increases the total amount of solar heat obtained during the day and stores excess solar energy to extend the operation time of solar heavy oil thermal recovery. Although it has a certain promoting effect on the increase of heavy oil production, increasing the energy field area also increases the equipment manufacturing cost and carbon emissions during the construction process. Summary of the invention
[0004] The purpose of the present invention is to address the shortcomings of the prior art, such as the large amount of natural gas consumption that reduces the energy-saving and emission-reduction effect of solar heavy oil thermal recovery, the increase in energy field area also increases the equipment manufacturing cost and carbon emissions during the construction process, the combustion causes a large amount of greenhouse gas emissions, and produces serious environmental problems, the heavy oil production is reduced, the economic profit is reduced, and the like. The present application provides a crop straw biomass chemical heat storage gel and a preparation method and application thereof. The biomass heat storage gel control agent uses common agricultural waste crop straw as a matrix, biopolymers as a cross-linking agent, carbonates as a chemical heat storage functional filler, and carbon materials as a thermal conductor. It has high heat storage capacity, carbon capture efficiency and environmental friendliness. When used as a control agent in solar steam flooding of heavy oil reservoirs, it can effectively solve the defects of poor heating continuity, low production efficiency and high carbon emissions of solar steam flooding.
[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0006] A method for preparing a crop straw biomass chemical heat storage gel comprises the following steps:
[0007] a) at 20° C. to 25° C., 50 wt% to 90 wt% of carbonate chemical heat storage filler, 0.5 wt% to 6 wt% of crop straw powder, 0.07 wt% to 0.5 wt% of carbon-based heat conductive filler, and 0.55 wt% to 4 wt% of biopolymer gelling agent are added into water under stirring at 600 rpm to 800 rpm, and stirred at a constant speed of 600 rpm to 800 rpm to effectively dissolve and disperse the above reaction raw materials to obtain a uniform suspension;
[0008] b) adding the biopolymer gelling agent dropwise to the suspension of step a) under stirring conditions at a stirring speed of 1000 rpm to 1500 rpm, and continuously stirring at a high speed of 1000 rpm to 1500 rpm for 45 min to 90 min to fully swell the biopolymer and obtain a sol with uniform viscosity;
[0009] c) The sol is sealed and allowed to stand at 65° C. to 90° C. for 48 h to 96 h to gel and age the sol, thereby obtaining a crop straw biomass chemical heat storage gel.
[0010] Furthermore, in step a), the carbonate chemical heat storage filler is MgCO3, NaCO3, K2CO3, CdCO3, ZnCO3 or PbCO3.
[0011] Furthermore, the crop straw powder in step a) is powder ground from wheat straw, rice straw, corn straw, sorghum straw, bean straw, cotton straw or rape straw.
[0012] Furthermore, the carbon-based thermally conductive filler in step a) is micro- or nano-particles of graphite, graphene, carbon fiber or carbon nanotube.
[0013] Furthermore, in step a), the biopolymer gelling agent is sodium alginate, guar gum, xanthan gum, hyaluronic acid, agar powder or konjac gum.
[0014] Furthermore, the crop straw powder in step a) is obtained by sequentially processing the crop straw through a straw crusher and a ball mill.
[0015] Furthermore, the particle size of the crop straw powder in step a) is 18 μm to 45 μm.
[0016] Furthermore, in the step a), the particle size of the crop straw powder is 325 mesh to 800 mesh.
[0017] A crop straw biomass chemical heat storage gel prepared by any of the above preparation methods.
[0018] The application also discloses the application of crop straw biomass chemical heat storage gel in solar steam flooding of heavy oil reservoirs.
[0019] Principle explanation: The preparation method of crop straw biomass chemical heat storage gel uses agricultural waste crop straw as the gel matrix and biopolymer as the physical cross-linking agent. The supramolecular combination between biopolymer and active components in crop straw (mainly cellulose and lignin) is used to construct a strong biomass gel network. At the same time, carbonate is used as the thermochemical heat storage functional filler to utilize its thermochemical reaction. The reversible transformation in the gel stores solar heat and captures CO2. In addition, the introduction of carbon-based microparticles (thermal conductors) provides an efficient heat transfer channel for the above-mentioned biomass heat storage gel, which makes the gel have a higher energy charging / heat release efficiency and indirectly improves its carbon capture efficiency.
[0020] Compared with the prior art, the beneficial effects of the present invention include:
[0021] 1. The crop straw biomass chemical heat storage gel prepared by the present invention can effectively enhance the sustainability of solar heating and improve the energy efficiency of solar heavy oil steam flooding process; compared with ordinary polymer gel flooding agent, the crop straw biomass chemical heat storage gel can increase the solar heavy oil steam flooding recovery rate by 30.8% and the energy efficiency by 221%;
[0022] 2. The carbonate functional filler in the crop straw chemical heat storage gel has a high heat storage capacity, which can make full use of the solar energy collected during the day for heavy oil thermal recovery at night, thereby extending the working time of solar heavy oil thermal recovery, making the solar steam flooding technology adaptable to all-weather oil recovery projects, and improving the production efficiency of solar heavy oil thermal recovery; compared with ordinary polymer gel flooding agents, the crop straw biomass chemical heat storage gel has latent heat storage capacity, and its heat storage capacity and heat storage efficiency are 1013 J·g -1 、2.03W·m -1 ·K -1 ;
[0023] 3. The injection of heat storage gel can improve the steam injection profile, alleviate steam cross-flow and gravity overburden, and thus reduce the ineffective heat loss of steam-based heavy oil thermal recovery;
[0024] 4. The crop straw chemical heat storage gel displacement agent prepared by the present invention can significantly reduce carbon emissions. The crop straw biomass chemical heat storage gel has a high carbon capture capacity and can absorb and fix a large amount of CO2 in the gel during the heat release process; 5. The solar heavy oil thermal recovery process based on the heat storage gel requires the injection of a large amount of CO2 into the formation. In addition to part of the gas that migrates with the produced heavy oil, a large amount of remaining CO2 is stored in the formation, which achieves further carbon capture and storage, effectively reduces carbon emissions, and is conducive to alleviating environmental crises; Compared with ordinary polymer gel displacement agents, the crop straw biomass chemical heat storage gel has carbon capture performance, and its CO2 adsorption capacity and CO2 adsorption rate are 37.4 mg·g -1 and 0.26mg·(g·min) -1 With the help of crop straw biomass chemical heat storage gel, the core can store 55 mg·mL of CO2. -1 ;
[0025] 6. The crop straw chemical heat storage gel prepared by the present invention has low biological hazard;
[0026] 7. The crop straw biomass chemical heat storage gel is composed of biomass (crop straw, biopolymer gelling agent) and low biotoxicity components (carbonate, carbon-based micron particles). It has high biodegradability and low biological hazards, which is beneficial to protecting the underground ecological environment. Compared with ordinary polymer gel adjustment and displacement agents, the crop straw biomass chemical heat storage gel can be completely biodegraded within 4 months, and can increase the wheat germination index by 16% and the number of earthworm offspring by 14%, which is beneficial to protecting the underground ecological environment during oil production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1The infrared spectra FTIR graphs of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application, the wheat straw powder in Comparative Example 3, and the sodium alginate in Comparative Example 4;
[0028] Figure 2 XRD diagrams of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application, the wheat straw powder in Comparative Example 3, and the sodium alginate in Comparative Example 4;
[0029] Figure 3 The Raman spectra of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application and the graphite powder in Comparative Example 5;
[0030] Figure 4 The X-ray photoelectron spectroscopy XPS graphs of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application and the wheat straw / sodium alginate / graphite high thermal conductivity biomass gel WS / SA / G in Comparative Example 1;
[0031] Figure 5 The scanning electron microscope (SEM) images of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application, the wheat straw biomass gel WS / SA in Comparative Example 2, and the wheat straw powder in Comparative Example 3;
[0032] Figure 6 Transmission electron microscope TEM images of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application, the wheat straw biomass gel WS / SA in Comparative Example 2, and the wheat straw powder in Comparative Example 3;
[0033] Figure 7 This is the element mapping diagram of C, O, and Mg elements of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application;
[0034] Figure 8 Thermogravimetric analysis TGA diagram of MgCO3 in comparative example 6 of the present application;
[0035] Fig. 9 This is the thermogravimetric analysis TGA graph of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application;
[0036] Fig.10The differential scanning calorimetry DSC graphs of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application, the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-70% in Example 2, the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-50% in Example 3, and MgCO3 in Control Example 6; Fig.11 The temperature-time curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application and the MgCO3 in the control example 6 in the simulation experiment;
[0037] Fig.12 The thermal conductivity-graphite content curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application and the wheat straw gel WS / SA in Comparative Example 2;
[0038] Fig.13 The temperature rise curves of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application and the wheat straw gel WS / SA in Comparative Example 2 in infrared thermal imaging analysis;
[0039] Fig.14 The heating rate-graphite content curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application and the wheat straw gel WS / SA in Comparative Example 2 in infrared thermal imaging analysis;
[0040] Fig.15 This is the infrared thermal imaging image of the wheat straw gel WS / SA in Comparative Example 2 of this application;
[0041] Fig.16 This is an infrared thermal imaging image of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application;
[0042] Fig.17 The differential scanning calorimetry DSC diagram of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% after 0 and 30 cycles of heating-cooling cycles in Example 1 of the present application;
[0043] Fig.18 The temperature-time curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application after 1 to 6 heating-cooling cycles in the simulation experiment;
[0044] Fig.19The CO2 adsorption curve (pure CO2 atmosphere) of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% at 80°C, 200°C, 300°C, and 400°C in Example 1 of the present application;
[0045] Fig. 20 The CO2 adsorption curve (80°C) of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application in a pure CO2 atmosphere and a 10% CO2+90% N2 atmosphere;
[0046] Fig.21 The cyclic CO2 adsorption / desorption curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application;
[0047] Fig. 22 This is the heat release-CO2 adsorption curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application;
[0048] Fig.23 This is the heavy oil recovery rate-injection time curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in the core displacement experiment in Example 1 of the present application;
[0049] Fig.24 This is the cumulative oil-gas ratio-injection time curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in the core displacement experiment in Example 1 of the present application;
[0050] Fig.25 This is the oil production energy consumption-injection time curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in the core displacement experiment in Example 1 of the present application;
[0051] Fig.26 This is the core temperature field diagram of the steam flooding of this application and the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% assisted steam flooding in Example 1;
[0052] Fig. 27 This is the CO2 storage capacity-injection time curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in the core displacement experiment in Example 1 of the present application;
[0053] Fig.28 The mass loss-time curve of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in the biodegradation experiment in Example 1 of the present application;
[0054] Fig.29 A bar graph of wheat germination index and wheat root length of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in a wheat germination experiment in Example 1 of the present application;
[0055] Fig.30 A bar graph showing the number of earthworm offspring and the average mass of earthworms in the animal toxicity test of the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% in Example 1 of the present application;
[0056] Fig.31 This application is a specific synthesis route for synthesizing crop straw biomass chemical heat storage gel in one step, using wheat straw as a biomass matrix, sodium alginate as a biopolymer gelling agent, carbonate as a chemical heat storage filler, and graphite as a thermal conductor. DETAILED DESCRIPTION
[0057] In view of the objectives, technical solutions and advantages of the present invention, the present invention is described in detail below in conjunction with embodiments and drawings.
[0058] In order to effectively improve the production efficiency and energy efficiency of solar heavy oil steam flooding and absorb carbon emissions in the industrial process, this patent designs and synthesizes a crop straw biomass chemical heat storage gel with both chemical heat storage and carbon capture functions. Compared with traditional gel adjustment and flooding agents, the crop straw biomass chemical heat storage gel has the following advantages for solar heavy oil steam flooding: 1) Good heat storage performance. The carbonate functional filler in the crop straw biomass chemical heat storage gel has a high heat storage capacity, which can make full use of the solar energy collected during the day for heavy oil thermal recovery at night, thereby extending the working time of solar heavy oil thermal recovery, making the solar heavy oil steam flooding technology adaptable to all-weather oil recovery projects, and improving the production and energy efficiency of the solar heavy oil thermal recovery process. In addition, the injection of heat storage gel can improve the steam injection profile, alleviate steam crossflow and gravity overburden, thereby reducing the ineffective heat loss of steam-based heavy oil thermal recovery. 2) Higher carbon capture capacity. The crop straw biomass chemical heat storage gel has a high carbon capture performance and can absorb and fix a large amount of CO2 in the gel during the heat release process. At the same time, the solar heavy oil thermal recovery process based on the heat storage gel requires the injection of a large amount of CO2 into the formation. In addition to some of the gas that migrates with the produced heavy oil, a large amount of remaining CO2 is stored in the formation, which achieves further carbon capture and storage, effectively reduces carbon emissions, and is conducive to alleviating environmental crises. 3) Strong environmental friendliness. The crop straw biomass chemical heat storage gel is composed of biomass (crop straw, biopolymer gelling agent) and low biotoxicity components (carbonate, carbon material), with high biodegradability and low biological hazards, which is conducive to protecting the underground ecological environment.
[0059] This patent uses easily degradable and environmentally friendly biomass raw materials (crop straw, biopolymer gelling agent) as the matrix, and carbonate as heat storage and carbon capture functional filler, to design and synthesize a biomass hydrogel with both chemical heat storage and carbon capture functions, and use it for regulation and drive. Specifically: the supramolecular interaction between crop straw (agricultural waste) and biopolymers (industrial by-products) is used to construct a highly elastic biomass network, and carbon-based micron particles are introduced into it as a thermal conductor to prepare a high thermal conductivity gel matrix. At the same time, carbonate is loaded as a heat storage functional filler in the above-mentioned gel matrix, and its reversible thermochemical changes at high temperature (300°C and above) and high CO2 partial pressure are used to enable the biomass chemical heat storage gel to store and release thermal energy at a specific temperature.
[0060] Example 1
[0061] A method for preparing crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, specifically comprising the following steps:
[0062] a) at 25° C., taking 90 wt % of carbonate chemical heat storage filler MgCO3, 1.2 wt % of wheat straw powder, 0.1 wt % of graphite heat conductive filler, and 0.8 wt % of sodium alginate gelling agent according to mass ratio, adding the MgCO3 chemical heat storage filler, wheat straw powder and graphite heat conductive filler into water under stirring at 800 rpm, stirring at a constant speed to effectively dissolve and disperse the above reaction raw materials to obtain a uniform suspension;
[0063] b) adding sodium alginate gelling agent dropwise to the suspension of step a) under stirring at a stirring speed of 1500 rpm, and continuously stirring at a high speed of 1500 rpm for 90 min to completely swell the sodium alginate biopolymer and obtain a sol with uniform viscosity;
[0064] c) The sol is sealed and allowed to stand at 80° C. for 96 hours to gel and age, thereby obtaining the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%.
[0065] Example 2
[0066] A method for preparing crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-70%, specifically comprising the following steps:
[0067] a) at 25° C., taking 70 wt % of carbonate chemical heat storage filler MgCO3, 3.6 wt % of wheat straw powder, 0.35 wt % of graphite heat conductive filler, and 2.8 wt % of sodium alginate gelling agent according to mass ratio, adding the MgCO3 chemical heat storage filler, wheat straw powder and graphite heat conductive filler into water under stirring at 800 rpm, stirring at a constant speed to effectively dissolve and disperse the above reaction raw materials to obtain a uniform suspension;
[0068] b) adding sodium alginate gelling agent dropwise into the suspension of step a) under stirring conditions at a stirring speed of 1200 rpm, and continuously stirring at a high speed of 1200 rpm for 60 min to completely swell the sodium alginate biopolymer and obtain a sol with uniform viscosity; c) sealing the sol and standing it at 80° C. for 65 h to gel and age it, thereby obtaining the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-70%.
[0069] Example 3
[0070] A method for preparing crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-50%, specifically comprising the following steps:
[0071] a) at 25° C., taking 50 wt % of carbonate chemical heat storage filler MgCO3, 6 wt % of wheat straw powder, 0.5 wt % of graphite heat conductive filler, and 4 wt % of sodium alginate gelling agent according to mass ratio, adding the MgCO3 chemical heat storage filler, wheat straw powder and graphite heat conductive filler into water under stirring at 600 rpm, stirring at a constant speed to effectively dissolve and disperse the above reaction raw materials to obtain a uniform suspension;
[0072] b) adding sodium alginate gelling agent dropwise to the suspension of step a) under stirring at a stirring speed of 1000 rpm, and continuously stirring at a high speed of 1000 rpm for 45 min to completely swell the sodium alginate biopolymer and obtain a sol with uniform viscosity;
[0073] c) The sol is sealed and allowed to stand at 70° C. for 48 hours to gel and age, thereby obtaining the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-50%.
[0074] Comparative Example 1
[0075] The preparation of wheat straw / sodium alginate / graphite high thermal conductivity biomass gel WS / SA / G is as follows:
[0076] (1) At 25° C., the wheat straw powder and the graphite thermal conductive filler were added to water at a concentration of 10 wt % and 1.2 wt % respectively, with stirring at 600 rpm, and the mixture was stirred at a constant speed to effectively dissolve and disperse the above reaction materials to obtain a uniform suspension;
[0077] (2) slowly adding the sodium alginate gelling agent to the suspension of step (1) at a concentration of 8 wt % under stirring at 1000 rpm, and continuing the high-speed stirring for 60 min to completely swell the sodium alginate biopolymer and obtain a sol with uniform viscosity;
[0078] (3) The sol was sealed and allowed to stand at 80° C. for 48 h to gel and age, thereby obtaining a wheat straw / sodium alginate / graphite high thermal conductivity biomass gel WS / SA / G.
[0079] Comparative Example 2
[0080] The preparation of wheat straw biomass gel WS / SA is as follows:
[0081] (1) adding wheat straw powder to water at 25° C. at a concentration of 10 wt % of wheat straw powder while stirring at 600 rpm, and stirring at a constant speed to fully disperse the wheat straw powder in the water to obtain a uniform suspension;
[0082] (2) slowly adding the sodium alginate gelling agent to the suspension of step (1) at a concentration of 8 wt % under stirring at 1000 rpm, and continuing the high-speed stirring for 45 min to completely swell the sodium alginate biopolymer and obtain a sol with uniform viscosity;
[0083] (3) The sol was sealed and allowed to stand at 80°C for 48 h to gel and age, thereby obtaining wheat straw biomass gel WS / SA.
[0084] Comparative Example 3
[0085] Wheat straw powder was used as a control example.
[0086] Comparative Example 4
[0087] Sodium alginate was used as a control example.
[0088] Comparative Example 5
[0089] Graphite powder is used as a control example.
[0090] Comparative Example 6
[0091] Take MgCO3 as a control example.
[0092] Infrared spectroscopy (FTIR) analysis of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, wheat straw powder and sodium alginate, see Figure 1 .like Figure 1As shown in the figure, compared with the FTIR spectra of wheat straw and sodium alginate, the characteristic peaks of wheat straw and sodium alginate coexist in the infrared spectrum of WS / SA / G@MgCO3-90% gel, and the peak position of the carboxyl-COO-stretching vibration peak belonging to sodium alginate changes, the free peak intensity of the hydroxyl stretching vibration and in-plane bending vibration belonging to sodium alginate and wheat straw weakens, the intensity of the association peak increases and the peak position changes, and the peak position of the COC stretching vibration peak belonging to sodium alginate and wheat straw changes, indicating that the cellulose and lignin components in sodium alginate form extensive and abundant hydrogen bonds with sodium alginate. Moreover, compared with wheat straw, the absorption peaks of the out-of-plane bending vibration and deformation vibration of the benzene ring CH of lignin in wheat straw in the infrared spectrum of WS / SA / G@MgCO3-90% gel are blue-shifted, indicating that the supramolecular coupling between the lignin component in wheat straw and sodium alginate weakens the hydrophobic association between lignin molecules and produces a plasticizing effect on lignin.
[0093] X-ray diffraction analysis (XRD) of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, wheat straw powder and sodium alginate, see Figure 2 .like Figure 2 As shown in the XRD spectrum, wheat straw and sodium alginate are both amorphous, and the cellulose in wheat straw shows diffraction peaks of methyl-modified cellulose chain and unmodified cellulose chain at 12.11° and 22.56°, respectively. After the cross-linking reaction is completed, the WS / SA / G@MgCO3-90% gel is amorphous, and the diffraction peak intensity of cellulose in wheat straw is weakened, and the peak position changes, indicating that there is a strong supramolecular bond between sodium alginate and cellulose components in wheat straw in the WS / SA / G@MgCO3-90% gel.
[0094] Raman spectroscopy analysis of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% and graphite, see Figure 3 .like Figure 3 As shown in the figure, the Raman spectra of WS / SA / G@MgCO3-90% gel are at 1572.9 cm -1 、1342.9cm -1 and 2705.3cm -1 The G peak, D peak and D* peak belonging to graphite appeared at D / I G =0.243, I D * / I G=0.505 are both close to pure graphite, indicating that the graphite particles loaded in WS / SA / G@MgCO3-90% gel still have a highly ordered crystal structure, and the graphite is mainly fixed in the gel by van der Waals force, which is conducive to the full play of its high thermal conductivity in the gel.
[0095] X-ray photoelectron spectroscopy (XPS) analysis of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% and wheat straw / sodium alginate / graphite high thermal conductivity biomass gel WS / SA / G, see Figure 4 .like Figure 4 As shown, compared with WS / SA / G gel, the XPS spectrum of WS / SA / G@MgCO3-90% gel simultaneously contains characteristic peaks of Mg1s, C1s and O1s, indicating that MgCO3 is successfully introduced into WS / SA / G@MgCO3-90% gel.
[0096] Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) analysis of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, wheat straw biomass gel WS / SA and wheat straw powder, see Figure 5 , Figure 6 .like Figure 5 , Figure 6 As shown, wheat straw contains a large number of lignin sheets and cellulose fiber bundles. As the cross-linking reaction proceeds, the lignin and cellulose inside the wheat straw are connected by hydrogen bonds with sodium alginate to form a tightly cross-linked biomass gel network. Compared with the wheat straw biomass gel WS / SA, the network surface of the crop straw chemical heat storage gel WS / SA / G@MgCO3-90% becomes rough, a large number of graphite and MgCO3 particles are attached to the gel surface, and many encapsulated inorganic salt crystals are found in the gel particles, indicating that graphite and MgCO3 are successfully introduced into the WS / SA biomass matrix and evenly distributed throughout the gel network.
[0097] Elemental mapping analysis of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, see Figure 7 .like Figure 7 As shown in the graph, in the WS / SA / G@MgCO3-90% gel, the C and O elements are concentrated in the gel network skeleton at the sampling site, while the Mg element is evenly distributed on the grid surface and internal pores of the gel network, indicating that graphite and MgCO3 are successfully introduced into the WS / SA biomass matrix and evenly distributed in the entire gel network.
[0098] Thermogravimetric analysis (TGA) and differential scanning calorimetry (DSC) of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, WS / SA / G@MgCO3-70%, WS / SA / G@MgCO3-50% and reference MgCO3, see Figure 8 , Fig. 9 , Fig.10 .like Figure 8 , Fig. 9 As shown, WS / SA / G@MgCO3-90% gel has a similar thermal decomposition / carbonation transition temperature to MgCO3 / MgO. At the same time, the above reaction enthalpy change in the gel is proportional to the amount of MgCO3 loaded, indicating that the coupling of the biomass matrix and the MgCO3 inorganic salt crystals in the gel does not have a significant effect on its thermochemical reaction characteristics. In addition, during the endothermic-exothermic process, the encapsulation rate and encapsulation efficiency of the WS / SA / G@MgCO3 thermal storage gel are similar to the mass percentage of MgCO3 inside it, and the heat storage capacity is as high as more than 90%, indicating that most of the carbonates loaded in the gel matrix participate in the thermochemical reaction during the transition from high temperature + N2 environment to low temperature + CO2 environment. In particular, the thermal decomposition / carbonation reaction enthalpy change, encapsulation rate, encapsulation efficiency and heat storage capacity of the WS / SA / G@MgCO3-90% gel are 1013 J·g -1 / 904J·g -1 , 85.1%, 85.4% and 99.6%, showing high heat storage performance. This is because, with the formation of the gel network skeleton and its attraction and restraint of the surrounding water molecules during the gelation process, the volume of the reaction system shrinks. Except for a small amount of MgCO3 particles that are sealed in the gel skeleton due to van der Waals forces and steric hindrance, most of the carbonate crystals are adsorbed on the surface of the gel network or distributed in its internal pores, and can fully contact with CO2 in the external environment, thereby producing a thermochemical reaction. On the other hand, Fig.10 As shown in the figure, compared with MgCO3, in the differential scanning calorimetry (DSC) spectrum, the thermal decomposition starting temperature of WS / SA / G@MgCO3 heat storage gel is lower, the carbonation starting temperature is slightly higher, and the peak width of the thermal decomposition and carbonation peaks is reduced (this trend becomes more obvious as the carbonate loading in the gel decreases). This is because the uniform dispersion of MgCO3 in the high thermal conductivity gel matrix greatly increases the heating area of the carbonate particles (the lower the carbonate content in the gel, the larger the overall thermal contact area of the carbonate), thereby accelerating and catalyzing the thermochemical reaction, thereby improving the heat storage / release efficiency of the MgCO3 crystals.
[0099] In order to simulate and analyze the heat storage performance of crop straw chemical heat storage gel WS / SA / G@MgCO3 under quasi-working environment, the crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% and reference MgCO3 were simulated and analyzed using thermostats, thermocouples and other experimental equipment. In the simulation experiment, the WS / SA / G@MgCO3-90% gel was placed at 500℃ and N2 environment for 12 hours, then cooled to 25℃, and CO2 was introduced into the thermostat to make its relative partial pressure reach 100% or 10% for 12 hours to analyze the heat storage / release performance of the gel under quasi-working environment. The analysis results are shown in Fig.11 .
[0100] like Fig.11 As shown in the figure, during the heating-cooling process, the temperature curve of WS / SA / G@MgCO3-90% gel is similar to that of MgCO3, and both exhibit similar thermal behaviors. Specifically, at 500℃, the internal temperature of the gel rises rapidly, and a temperature platform appears at about 303℃ (due to the thermal decomposition reaction of MgCO3); at low temperatures, the gel temperature drops slowly, and its internal temperature remains above 150℃ after cooling for 12h, and an exothermic peak of MgO carbonation reaction appears at 450℃, proving that WS / SA / G@MgCO3-90% gel still has good heat storage / release efficiency under quasi-working conditions. In addition, compared with MgCO3, the heating and cooling rate of WS / SA / G@MgCO3-90% gel is significantly accelerated, the thermal degradation temperature is lowered, and the peak width of the carbonation exothermic peak is reduced, which once again proves that the high thermal conductivity gel matrix encapsulates carbonates effectively catalyzes their thermochemical reactions, so that the composite gel exhibits higher heat absorption / release efficiency.
[0101] Thermal conductivity test and infrared thermal imaging analysis of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% and reference wheat straw biomass gel WS / SA, see Fig.12 , Fig.13 , Fig.14 , Fig.15 , Fig.16 .like Fig.12 , Fig.13 , Fig.14 , Fig.15 , Fig.16 As shown in the figure, under constant temperature heating at 350℃, compared with the wheat straw biomass gel WS / SA, the heating rate of WS / SA / G@MgCO3-90% gel is greatly improved, and with the gradual increase of graphite content, the thermal conductivity and heating rate of the gel (infrared thermal imaging analysis) are significantly improved, indicating that the graphite component in WS / SA / G@MgCO3-90% gel is the decisive factor affecting its thermal conductivity, and the high thermal conductivity of the gel comes from the high thermal conductivity channels formed by its internal graphite sheets.
[0102] Cyclic DSC test and cyclic heating-cooling experimental analysis of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, see Fig.17 , Fig.18 After 30 cycles of heating-cooling, the reaction enthalpy of WS / SA / G@MgCO3-90% increased from 1013 J·g -1 / 904J·g -1 Reduced to 973 J·g -1 / 868J·g -1 , the decrease was only 3.9% and 4.0%; at the same time, its temperature curve changed slightly (thermal decomposition temperature platform and carbonation exothermic peak remained basically unchanged), and the gel temperature remained at 116°C after cooling for 12 hours, indicating that the thermochemical heat storage of WS / SA / G@MgCO3-90% has high thermal reliability. In summary, considering the heat storage capacity, heat storage / heat release efficiency and thermal reliability of the gel, WS / SA / G@MgCO3-90% gel is selected as the best sample.
[0103] The CO2 adsorption-time curve, chemical heat release-CO2 adsorption curve and carbon capture performance cycle stability test of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% are shown in Fig.19 , Fig. 20 , Fig.21 , Fig. 22 .like Fig.19 As shown in the figure, as the ambient temperature drops from 400℃ to 80℃, the adsorption capacity of WS / SA / G@MgCO3-90% gel for CO2 gradually increases, and the adsorption rate decreases significantly, indicating that lowering the temperature within a specific temperature range can increase the degree of reaction of MgO+CO2→MgCO3, but will reduce its reaction rate. The adsorption capacity and adsorption rate of WS / SA / G@MgCO3-90% gel for CO2 at 400℃~80℃ are 9.6mg·g -1 ~37.4mg·g -1 and 0.26mg·(g·min) -1 ~0.9mg·(g·min) -1 , showing good CO2 adsorption performance. Fig. 20 As shown in Figure 2, compared with pure CO2 atmosphere, in the environment of 10% CO2 + 90% N2, the relative adsorption capacity of CO2 by WS / SA / G@MgCO3 gel still remained at 92%, reaching 34.5 mg·g -1 , indicating that WS / SA / G@MgCO3 gel has a high selectivity for the adsorption of CO2. In addition, according to the cyclic adsorption test, Fig.21As shown in the figure, after 30 heating-cooling cycles, the adsorption / desorption capacity and rate of WS / SA / G@MgCO3-90% gel for CO2 still remain at 77% and 85% of the original, indicating that the thermal storage gel has good cyclic stability for the adsorption of CO2. Fig. 22 As shown, the amount of CO2 adsorbed by WS / SA / G@MgCO3-90% gel is linearly correlated with the amount of heat released, indicating that the heat storage gel supplies heat to the outside world mainly through the thermochemical reaction of the MgCO3 crystals loaded inside it.
[0104] In order to analyze the optimization effect and mechanism of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90% on the sustainability of solar steam drive heating, heavy oil thermal recovery yield and energy consumption, a simulated solar steam drive core displacement experiment was carried out, and the temperature field distribution inside the core during the steam drive process was visualized using thermocouples. In the core displacement experiment, the heavy oil saturated core was first steam driven at 500℃ for 12h, during which WS / SA / G@MgCO3-90% heat storage gel was injected and the steam heat was used to charge the gel; then 25℃ CO2 was continuously injected into the core to drive oil again for 12h, and the analysis results are shown in Fig.23 , Fig.24 , Fig.25 .
[0105] like Fig.23 , Fig.24 , Fig.25 As shown in the figure, the injection and adjustment of crop straw chemical heat storage gel WS / SA / G@MgCO3-90% greatly increased the crude oil recovery rate of steam drive. At the same time, during the CO2 drive process at room temperature, without the help of external heat source, the CO2 fluid heated by WS / SA / G@MgCO3-90% gel effectively heated and displaced the residual oil in a large range of the core, and its relative recovery rate reached 25.6% OOIP (corresponding to residual oil saturation), which is 79% of the relative recovery rate of steam drive, showing a high thermal recovery potential. At the same time, compared with the high-energy consumption steam drive, the energy consumption of gel-heated CO2 drive was reduced by 68.8%, reaching 57J·(mL oil) -1 The cumulative oil-gas ratio (COSR) increased by 267% to 0.66 mL·mL -1, showing higher energy efficiency. The high recovery rate and energy efficiency ratio of the "high-temperature steam flooding powered by solar energy during the day + CO2 heated by gel at night" oil recovery mode are mainly due to: 1) The high heat storage performance of WS / SA / G@MgCO3-90% gel flooding agent significantly improves the continuity of solar heating. The loading of high-performance thermochemical heat storage filler MgCO3 and high thermal conductivity graphite particles gives WS / SA / G@MgCO3-90% gel a higher heat storage capacity and heat absorption / heat release efficiency, so that the gel can quickly absorb the heat of high-temperature solar steam during the day and heat the displacement fluid at night, thereby realizing 7 / 24 all-weather heavy oil production completely heated by solar energy, while maintaining the high recovery rate of heavy oil thermal recovery and effectively reducing its energy consumption. 2) WS / SA / G@MgCO3-90% gel with good thermal conductivity greatly enhances the steam oil recovery capacity. WS / SA / G@MgCO3-90% gel effectively improves the steam injection profile, greatly increases its swept area, and thus significantly improves the steam oil recovery capacity. At the same time, the high thermal conductivity of WS / SA / G@MgCO3-90% gel makes it an efficient heat transfer medium, which significantly enhances the heat transfer of steam to heavy oil and alleviates the decrease in steam drive efficiency caused by thermal retardation.
[0106] Analysis of core temperature field of steam flooding of crop straw biomass chemical heat storage gel WS / SA / G@MgCO3-90%, see Fig.26 .like Fig.26 As shown in the figure, during the high-temperature steam flooding process, the injection of WS / SA / G@MgCO3-90% thermal storage gel significantly expanded the effective heating area of steam (500℃~200℃, red / yellow (heating zone) and green area (heating zone)), indicating that the thermal storage gel effectively adjusted the steam injection profile (increased the steam sweep area) and enhanced the heat transfer of steam to heavy oil, thereby enhancing its oil recovery capacity. At the same time, during the normal temperature CO2 flooding process, without the help of external heat source, the CO2 fluid heated by WS / SA / G@MgCO3-90% gel effectively heated and displaced the residual oil in a large range in the core, and its effective heating area was as high as 69.4%, showing a high thermal recovery potential.
[0107] Core carbon storage performance test of crop straw chemical heat storage gel flooding agent WS / SA / G@MgCO3-90% assisted steam flooding, see Fig. 27 .like Fig. 27 As shown in the figure, as the WS / SA / G@MgCO3-90% gel thermal CO2 flooding proceeds, the injected CO2 diffuses in the core and is largely sealed in the core pore throats. After 12 hours of flooding, the CO2 reserves of the artificial core are as high as 55 mg mL -1, showing a high carbon capture capacity, indicating that the oil production mode of "steam drive with solar heating + CO2 drive with thermochemical heat storage gel heating" can not only significantly improve the energy efficiency of thermal recovery of heavy oil, but also make full use of strata with developed pore structures (porous media) as natural storage bins, capture and seal a large amount of CO2 emitted in daily life and industrial production, which is conducive to achieving carbon neutrality in oil production projects.
[0108] Analysis on the environmental friendliness of crop straw chemical heat storage gel flooding agent WS / SA / G@MgCO3-90%, see Fig.28 , Fig.29 , Fig.30 .like Fig.28 As shown in the figure, WS / SA / G@MgCO3-90% gel can be completely degraded naturally within 4 months, and its degradation products are mainly humic acid, showing good bioavailability and biodegradability. Fig.29 As shown in the figure, compared with water culture medium, the germination index and average seedling root length of wheat seeds in water-saturated WS / SA / G@MgCO3-90% gel culture medium increased by 16% and 85%, reaching 116% and 11.5 cm, respectively. Fig.30 As shown, compared with the untreated soil, the earthworms are obviously closer to the soil doped with WS / SA / G@MgCO3-90% gel (the approach rate is 33.3%), and after 14 days of cultivation, the earthworms have a higher number of offspring and average weight in the soil fertilized by gel. The above experimental phenomena show that WS / SA / G@MgCO3-90% gel has low biological toxicity and can effectively promote the growth and metabolism of plants and animals. This is because: 1) The MgCO3 crystals loaded in the gel have low toxicity and always exist in solid form, which has little harm to organisms. 2) The gel has high bioavailability, and the WS / SA / G biomass matrix inside it can provide rich nutrients and biochar for plants and animals in the soil, thereby promoting their growth. In addition, the degradation products of the gel are mainly humic acid, which can be used as a fertilizer to improve soil activity.
[0109] The crop straw biomass chemical heat storage gel prepared by the present invention has a multi-level "functional network + matrix network structure". Its internal carbonate functional network enables the gel to have both high heat storage capacity and carbon capture capacity. The carbon-based permeation network constructs a high-speed heat conduction channel covering the entire gel, improving the gel's heat storage and carbon capture efficiency, while the physically cross-linked high-strength biomass matrix network provides effective structural support and protective support for the functional network in the gel, giving the gel good adjustment and flooding performance. The core displacement experiment results show that the "daytime solar heating steam flooding + nighttime crop straw chemical heat storage gel heating CO2 flooding" oil recovery method effectively improves the production efficiency of solar heavy oil steam flooding, reduces the energy consumption of heavy oil thermal recovery, and increases the reuse rate of CO2 waste gas, which is conducive to the clean production of heavy oil.
[0110] In summary, the crop straw chemical heat storage gel flooding agent of the present invention has the following advantages: 1) Strong heat storage capacity, which can effectively enhance the sustainability of solar heating and improve the production efficiency of solar heavy oil steam flooding. The carbonate functional filler in the crop straw chemical heat storage gel has a high heat storage capacity, which can make full use of the solar energy collected during the day for heavy oil thermal recovery at night, thereby extending the working time of solar heavy oil thermal recovery, making the solar steam flooding technology adaptable to all-weather oil recovery projects, and improving the production efficiency of solar heavy oil thermal recovery. 2) Strong carbon capture capacity, which is conducive to achieving carbon neutrality in heavy oil thermal recovery. The crop straw biomass chemical heat storage gel has a high carbon capture capacity and can absorb and fix a large amount of CO2 in the gel during the heat release process. At the same time, the solar heavy oil thermal recovery process based on the heat storage gel needs to inject a large amount of CO2 into the formation. In addition to some of the gas that migrates with the produced heavy oil, a large amount of remaining CO2 is stored in the formation, which realizes further carbon capture and storage, effectively reduces carbon emissions, and is conducive to alleviating environmental crises. 3) Environmentally friendly. The crop straw biomass chemical heat storage gel is composed of biomass (crop straw, biopolymer gelling agent) and low biotoxicity components (carbonate, carbon-based micron particles). It has high biodegradability and low biological hazards, and is beneficial to protecting the underground ecological environment.
[0111] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for preparing a crop straw biomass chemical heat storage gel, characterized in that: The steps include: a) at 20° C. to 25° C., 50 wt% to 90 wt% of carbonate chemical heat storage filler, 0.5 wt% to 6 wt% of crop straw powder, 0.07 wt% to 0.5 wt% of carbon-based heat conductive filler, and 0.55 wt% to 4 wt% of biopolymer gelling agent are added into water under stirring at 600 rpm to 800 rpm, and stirred at a constant speed of 600 rpm to 800 rpm to effectively dissolve and disperse the above reaction raw materials to obtain a uniform suspension; b) adding the biopolymer gelling agent dropwise to the suspension of step a) under stirring conditions at a stirring speed of 1000 rpm to 1500 rpm, and continuously stirring at a high speed of 1000 rpm to 1500 rpm for 45 min to 90 min to fully swell the biopolymer and obtain a sol with uniform viscosity; c) The sol is sealed and allowed to stand at 65° C. to 90° C. for 48 h to 96 h to gel and age the sol, thereby obtaining a crop straw biomass chemical heat storage gel.
2. The method for preparing a crop straw biomass chemical heat storage gel according to claim 1, characterized in that: In the step a), the carbonate chemical heat storage filler is MgCO3, NaCO3, K2CO3, CdCO3, ZnCO3 or PbCO3.
3. The method for preparing a crop straw biomass chemical heat storage gel according to claim 1, characterized in that: The crop straw powder in step a) is powder ground from wheat straw, rice straw, corn straw, sorghum straw, bean straw, cotton straw or rape straw.
4. The method for preparing a crop straw biomass chemical heat storage gel according to claim 1, characterized in that: In step a), the carbon-based thermally conductive filler is micro- or nano-particles of graphite, graphene, carbon fiber or carbon nanotube.
5. The method for preparing a crop straw biomass chemical heat storage gel according to claim 1, characterized in that: The biopolymer gelling agent in step a) is sodium alginate, guar gum, xanthan gum, hyaluronic acid, agar powder or konjac gum.
6. The method for preparing a crop straw biomass chemical heat storage gel according to claim 1, characterized in that: The crop straw powder in step a) is obtained by sequentially processing the crop straw through a straw crusher and a ball mill.
7. The method for preparing the crop straw biomass chemical heat storage gel according to claim 6, characterized in that: The particle size of the crop straw powder in step a) is 18 μm to 45 μm.
8. The method for preparing the crop straw biomass chemical heat storage gel according to claim 6, characterized in that: The particle size of the crop straw powder in step a) is 325 mesh to 800 mesh.
9. A crop straw biomass chemical heat storage gel prepared by any preparation method of claims 1 to 8.
10. Use of the crop straw biomass chemical heat storage gel according to claim 9 in solar steam flooding of heavy oil reservoirs.