Uniform long-wave infrared quantum dot, preparation method thereof and photoelectric detector
By controlling the concentration and injection time of selenourea and selenium disulfide precursors, the method achieves uniform long-wave infrared quantum dots with improved absorption characteristics for photoelectric detectors.
Patent Information
- Application Number
- CN202311833740.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-12-03
AI Technical Summary
Existing long-wave infrared quantum dot synthesis methods result in uneven size and morphology, which affects their performance in detection applications.
A method involving the use of selenourea as a selenium source precursor for nucleation and selenium disulfide for growth, with precise control over concentration, injection time, and reaction conditions to achieve uniform long-wave infrared quantum dots.
The method produces quantum dots with uniform size and morphology, extending their absorption range to long-wave and very long-wave infrared bands, enhancing their suitability for photoelectric detectors.
Smart Images

Figure CN119060732A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of long-wave infrared quantum dots, and in particular to a uniform long-wave infrared quantum dot and a preparation method thereof and a photoelectric detector. Background Art
[0002] Generally speaking, the infrared bands are divided into short-wave infrared (SWIR, 1-3μm), medium-wave infrared (MWIR, 3-5μm), long-wave infrared (LWIR, 8-14μm), and very long-wave infrared (VLWIR, >14μm). Any object that is not at absolute zero will radiate electromagnetic waves, and detecting the radiated electromagnetic waves can detect the object. According to Planck's blackbody radiation law, it is calculated that the energy density of blackbody radiation is proportional to the temperature. The temperature of most celestial bodies in the universe is very low, and the radiation energy density of low-temperature targets is very weak. Observing these celestial targets requires long-wave or even longer-wave infrared detectors.
[0003] The relevant long-wave infrared detection is mainly based on mercury cadmium telluride (HgCdTe) materials, quantum wells (QWs) and type II superlattice structures. They have the advantages of large light response, fast response speed, continuously adjustable band, mature and stable process, but they also face many challenges such as difficulty in realizing curved surface detection, inability to prepare large arrays and complex integration process. HgSe quantum dot materials have been widely studied based on their narrow-band absorption characteristics of intra-band transitions, flexible curved surface detection, good circuit compatibility, and the prospect of large-scale preparation. A synthesis of HgSe quantum dots is disclosed in the relevant documents, specifically dissolving Hg(OAc)2 in oleic acid and oleylamine, and adjusting the temperature between 60 and 120°C according to the expected final nanocrystal size. At the same time, SeS2 is dissolved in oleylamine under ultrasound and then injected into the reaction.
[0004] Regarding the above-mentioned related technologies, there is a problem of uneven size and morphology under the condition of meeting the size requirements of long-wave infrared. Summary of the invention
[0005] In order to improve the uniformity of quantum dot size and morphology while meeting the size requirements of long-wave infrared, the purpose of this application is to provide a uniform long-wave infrared quantum dot and a preparation method and a photoelectric detector.
[0006] In the first aspect, the preparation method of uniform long-wave infrared quantum dots provided in the present application adopts the following technical scheme:
[0007] A method for preparing uniform long-wave infrared quantum dots comprises the following steps:
[0008] Prepare 0.07-0.1 mol / L mercury precursor solution;
[0009] Prepare 0.4-0.6 mol / L selenourea solution, inject mercury precursor solution, react at 120-150° C. for 2-10 min to obtain a first solution, wherein the volume ratio of selenourea solution to mercury precursor solution is 1:20-30;
[0010] A 0.025-0.06 mol / L selenium disulfide solution is prepared, and the selenium disulfide solution is uniformly injected into the first solution at 120-150° C., and the injection time is controlled to be 15-40 min to obtain a second solution, wherein the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:0.5-1.2;
[0011] The second solution is purified to obtain uniform long-wave infrared quantum dots.
[0012] By adopting the above technical scheme, using selenourea solution as the selenium source precursor for nucleation and selenium disulfide as the selenium source precursor for growth, and comprehensively controlling the concentration and injection time, the absorption range of the synthesized quantum dot material is extended to the long wave band and even the very long wave band, and the size and morphology are uniform.
[0013] Optionally, the concentration of the mercury precursor solution is 0.075-0.09 mol / L, the concentration of the selenourea solution is 0.45-0.55 mol / L, and the volume ratio of the selenourea solution to the mercury precursor solution is 1:22-26.
[0014] By adopting the above technical solution, the concentration and volume ratio of the mercury precursor solution and selenourea are regulated to promote the initial nucleation amount and nucleation uniformity.
[0015] Optionally, the concentration of the mercury precursor solution is 0.083 mol / L, the concentration of the selenourea solution is 0.5 mol / L, and the volume ratio of the selenourea solution to the mercury precursor solution is 1:24.
[0016] By adopting the above technical solution, the concentration and volume ratio of mercury precursor solution and selenourea can be further regulated to promote the initial nucleation amount and nucleation uniformity, and the process of the entire reaction is stable, and the effect of preparing products in multiple batches is stable.
[0017] Optionally, the reaction time of the selenourea solution and the mercury precursor solution is 2.5-3.5 min.
[0018] By adopting the above technical solution, the nucleation effect is achieved while reducing the reaction time.
[0019] Optionally, the reaction temperature is 128-132°C.
[0020] By adopting the above technical solution, the reaction temperature can be further controlled, the growth nucleation effect can be comprehensively regulated, the uniformity of the final product can be promoted, and the process can be more stable.
[0021] Optionally, a 0.045-0.055 mol / L selenium disulfide solution is prepared, and the injection time is controlled to be 18-22 min when the selenium disulfide solution is uniformly injected into the first solution, and the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:0.8-1.2.
[0022] By adopting the above technical solution, a 0.05 mol / L selenium disulfide solution is prepared, and the selenium disulfide solution is uniformly injected into the first solution while the injection time is controlled to be 20 minutes, and the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:1.
[0023] Optionally, when the selenium disulfide solution is uniformly injected into the first solution, the injection time is controlled to be 20 minutes, and the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:1.
[0024] By adopting the above technical solution, the injection time and injection volume of the selenium disulfide solution are further controlled to meet the concentration ratio requirement between the selenium disulfide and the mercury source, thereby promoting better use of selenium disulfide for growth and promoting process stability.
[0025] Optionally, the injection is followed by a continuous reaction for 8-12 minutes.
[0026] By adopting the above technical solution, after the injection of selenium disulfide solution is completed, the aging reaction is continued for 8-12 minutes so that small-sized quantum dots are more inclined to dissolve, while large-sized quantum dots are more inclined to grow, thereby making the size and morphology of the quantum dots more uniform under the size condition that meets the long-wave infrared requirements.
[0027] In the second aspect, the uniform long-wave infrared quantum dots provided in this application adopt the following technical solutions:
[0028] The uniform long-wave infrared quantum dots are prepared by using the uniform long-wave infrared quantum dots preparation method.
[0029] By adopting the above technical solution, the long-wave infrared quantum dots prepared by the uniform long-wave infrared quantum dot preparation method have good uniformity in quantum dot size and morphology under the condition of meeting the size requirements of the long-wave infrared.
[0030] In a third aspect, the photoelectric detector provided in this application adopts the following technical solution:
[0031] A photoelectric detector comprises the uniform long-wave infrared quantum dots.
[0032] By adopting the above technical solution, uniform long-wave infrared quantum dots are applied to photoelectric detectors, thereby improving the application effect of photoelectric detectors and making them more useful in space systems such as space-based detection and meteorological monitoring.
[0033] In summary, the present application includes at least one of the following beneficial technical effects:
[0034] 1. Using selenourea solution as a selenium source precursor for nucleation and selenium disulfide as a selenium source precursor for growth, the concentration and injection time are comprehensively regulated, and the absorption range of the synthesized quantum dot material extends to the long-wave band, and even the very long-wave band, and the size and morphology are uniform; further regulating the relationship between the three (mercury source precursor, selenourea solution, selenium disulfide solution), such as concentration, volume, injection, etc., to obtain a stable preparation process;
[0035] 2. After the injection of the selenium disulfide solution is completed, the aging reaction is continued for 8-12 minutes so that small-sized quantum dots are more likely to dissolve, while large-sized quantum dots are more likely to grow, thereby making the quantum dots more uniform in size and morphology while meeting the size requirements of the long-wave infrared. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the process of preparing long-wave infrared quantum dots described in the embodiment of the present application;
[0037] Figure 2 is the Fourier infrared absorption spectrum of the uniform long-wave infrared quantum dots prepared in Example 1 of the present application;
[0038] Figure 3 is the Fourier infrared absorption spectrum of the uniform long-wave infrared quantum dots prepared in Example 2 of the present application;
[0039] Figure 4 It is the Fourier infrared absorption spectrum of the uniform long-wave infrared quantum dots prepared in Examples 3-4 of the present application;
[0040] Figure 5 It is the Fourier infrared absorption spectrum of the uniform long-wave infrared quantum dots prepared in Examples 5-7 of the present application;
[0041] Figure 6 is the Fourier infrared absorption spectrum of the uniform long-wave infrared quantum dots prepared in Example 8 of the present application;
[0042] Figure 7 is the Fourier infrared absorption spectrum of the quantum dots prepared in Comparative Example 1 of the present application;
[0043] Figure 8 This is the Fourier infrared absorption spectrum of the quantum dots prepared in Comparative Example 2 of the present application;
[0044] Fig. 9 This is the Fourier infrared absorption spectrum of the quantum dots prepared in Comparative Example 3 of the present application;
[0045] Fig.10is the Fourier infrared absorption spectrum of the quantum dots prepared in Comparative Example 4 of the present application;
[0046] Fig.11 It is the Fourier infrared absorption spectrum of the quantum dots prepared in Comparative Example 6 of the present application under filtered and unfiltered conditions;
[0047] Fig.12 is the Fourier infrared absorption spectrum of the quantum dots prepared in Comparative Example 7 of the present application;
[0048] Fig.13 is the Fourier infrared absorption spectrum of the quantum dots prepared in Comparative Example 8 of the present application;
[0049] Fig.14 It is a TEM image and particle size distribution diagram of uniform long-wave infrared quantum dots prepared in Example 1 of the present application;
[0050] Fig.15 This is a TEM image and particle size distribution diagram of uniform long-wave infrared quantum dots prepared in Example 2 of the present application;
[0051] Fig.16 It is a TEM image and particle size distribution diagram of uniform long-wave infrared quantum dots prepared in Example 6 of the present application;
[0052] Fig.17 It is the TEM image and particle size distribution diagram of the quantum dots prepared in Comparative Example 4 of the present application;
[0053] Fig.18 This is a TEM image of the quantum dots prepared in Comparative Example 5 of the present application;
[0054] Fig.19 TEM images of quantum dots prepared in Comparative Example 6 of the present application under filtered and unfiltered conditions;
[0055] Fig. 20 It is the TEM image and particle size distribution diagram of the quantum dots prepared in Comparative Example 7 of the present application;
[0056] Fig.21 It is the TEM image and particle size distribution diagram of the quantum dots prepared in Comparative Example 8 of the present application. DETAILED DESCRIPTION
[0057] In order to improve the photoelectric conversion efficiency of colloidal quantum dot devices, halogen elements are often used as ligand molecules in related technologies to achieve a good ligand passivation effect. However, the applicant found that the colloidal quantum dot precursor film obtained by colloidal quantum dot coating with metal halide as ligand exchange will decompose under the action of strong light, crystallize under the action of high temperature, and undergo ion migration under the action of strong electric field, which seriously restricts the high temperature, electric field, and radiation stability of the colloidal quantum dot device; the present application is drawn on this basis.
[0058] The present application embodiment provides a method for preparing uniform long-wave infrared quantum dots, referring to Figure 1 , including the following steps:
[0059] Prepare a 0.07-0.1 mol / L mercury precursor solution, wherein the mercury precursor solution can be prepared with oleic acid as a solvent (OLA), the mercury precursor can be specifically at least one of mercuric chloride (HgCl2) and mercuric acetate (Hg(OAc)2), and the dissolution temperature can be specifically 120-150°C, preferably 130°C;
[0060] Prepare a 0.4-0.6 mol / L selenourea solution, wherein the selenourea solution can be prepared with oleic acid as a solvent (OLA), the dissolution temperature can be 200-240° C., and the dissolution time is controlled to be at least completely dissolved, preferably 220° C., and the dissolution time is 2 hours;
[0061] The selenourea solution is injected into the mercury precursor solution at 120-150° C., and the reaction is carried out for 2-10 minutes to obtain a first solution, wherein the volume ratio of the selenourea solution to the mercury precursor solution is 1:20-30. In this step, the injection time is relatively short, which is a rapid injection operation, and the injection time can be specifically limited to no more than 3 seconds;
[0062] Prepare a 0.04-0.06 mol / L selenium disulfide solution, wherein the selenourea solution can be prepared with oleic acid as a solvent (OLA), the dissolution temperature can be 130-150° C., and the dissolution time is controlled to be at least completely dissolved, preferably 140° C., and the dissolution time is 1 hour;
[0063] The selenium disulfide solution is uniformly injected into the first solution at 120-150° C., and the injection time is controlled to be 15-40 minutes. After the injection is completed, the reaction is stopped to obtain a second solution, wherein the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:0.5-1.2. The method for stopping the reaction can be specifically injecting a cooling liquid into the reaction solution. The cooling liquid can be tetrachloroethylene (TCE), n-octane (OCT) and toluene, etc. In the initial stage of the preparation of long-wave infrared quantum dots, the cooling liquid can be placed on a refrigeration platform for cooling, that is, after the reaction time is over, the cooling liquid is quickly poured into the reaction solution, and the reaction solution stops reacting due to rapid cooling;
[0064] The second solution is purified to obtain uniform long-wave infrared quantum dots. After the synthesis reaction is completed, a large amount of unreacted mercury precursor, selenourea and selenium disulfide remain in the solution. These residues will have an adverse effect on the subsequent device performance. Generally, multiple purifications are performed to achieve the effect of purifying the quantum dots. The specific purification method may include the following steps:
[0065] S1. Using ethanol as an anti-solvent to precipitate the quantum dots, and then centrifuging to obtain a precipitate. The anti-solvent is usually a solvent with a strong polarity, such as methanol and acetone;
[0066] S2, dispersing the precipitate through a benign solvent, wherein the benign solvent may be n-octane (OCT), to obtain a dispersed solution;
[0067] S3. The dispersed solution is filtered to obtain a uniform long-wave infrared quantum dot solution. The filtration can be performed by using a syringe (with a flat-head needle) to take the quantum dot solution, and then filtering it with a green filter head.
[0068] In some embodiments, the concentration of the mercury precursor solution is 0.075-0.09 mol / L, the concentration of the selenourea solution is 0.45-0.55 mol / L, and the volume ratio of the selenourea solution to the mercury precursor solution is 1:22-26.
[0069] In some embodiments, the concentration of the mercury precursor solution is 0.083 mol / L, the concentration of the selenourea solution is 0.5 mol / L, and the volume ratio of the selenourea solution to the mercury precursor solution is 1:24.
[0070] In certain embodiments, the reaction time of the selenourea solution and the mercury precursor solution is 2.5-3.5 min.
[0071] In certain embodiments, the reaction temperature is 128-132°C, preferably 130°C.
[0072] In some embodiments, a 0.045-0.055 mol / L selenium disulfide solution is prepared, and the selenium disulfide solution is uniformly injected into the first solution for a controlled injection time of 18-22 min, and the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:0.8-1.2.
[0073] In some embodiments, a 0.05 mol / L selenium disulfide solution is prepared, and the selenium disulfide solution is uniformly injected into the first solution for a controlled injection time of 20 min, and the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:1.
[0074] In certain embodiments, the reaction is continued for 8-12 minutes after the injection is completed.
[0075] Furthermore, the embodiments of the present application provide a uniform long-wave infrared quantum dot prepared by the above-mentioned preparation method, and a photoelectric detector including the uniform long-wave infrared quantum dot.
[0076] The present application is further described in detail below in conjunction with embodiments.
[0077] Example 1
[0078] A method for preparing uniform long-wave infrared quantum dots, referring to Figure 1 , including the following steps:
[0079] Step 1: Prepare 0.083 mol / L mercury precursor solution (HgCl2 precursor solution). Specifically, weigh 136 mg (0.5 mmol) of HgCl2 precursor as a Hg source and dissolve it in 6 ml of oleylamine (OLA), stir and heat to 130°C and keep it stable (50 ml glass bottle);
[0080] Step 2: Prepare 0.5 mol / L selenourea solution. Specifically, weigh 123 mg (1 mmol) of selenourea precursor as a Se source and dissolve it in 2 ml of OLA to obtain a selenourea solution. The dissolution temperature is 220° C. and the dissolution time is 2 h.
[0081] Step 3, nucleation: 0.25 ml of selenourea solution was rapidly injected into the mercury precursor solution at 130° C. and reacted for 3 minutes to obtain a first solution;
[0082] Step 4: prepare a 0.05 mol / L selenium disulfide solution. Specifically, weigh 143 mg (1 mmol) of SeS2 precursor and dissolve it in 20 ml of OLA to obtain a selenium disulfide solution (SeS2 solution). The dissolution temperature is 140° C. and the reaction time is 1 h.
[0083] Step 5, growth: 8 ml of selenium disulfide solution is drawn into a 10 ml syringe, and the syringe is placed on a syringe pump. At 130° C., the injection rate is set to 0.3 ml / min to inject the selenium disulfide solution into the first solution for 20 min (a total of 6 ml of selenium disulfide solution is injected). After the injection is completed, 12 ml of tetrachloroethylene (TCE) is injected into the reaction solution as a cooling liquid to stop the reaction, thereby obtaining a second solution;
[0084] Step 6: Purifying the second solution to obtain uniform long-wave infrared quantum dots, specifically comprising:
[0085] S1. Use ethanol as an anti-solvent to precipitate the quantum dots, then separate them into two tubes and place them in a centrifuge for centrifugation (6000 rpm, 2 min), and remove the supernatant to obtain the precipitate;
[0086] S2, dispersing the precipitate with a benign solvent n-octane (OCT), and fully oscillating to completely disperse the quantum dots to obtain a dispersed solution;
[0087] S3. The dispersed solution is filtered to obtain a uniform long-wave infrared quantum dot solution. Specifically, the quantum dot solution can be taken with a syringe (equipped with a flat-head needle) and then filtered with a green filter head.
[0088] Example 2
[0089] A method for preparing uniform long-wave infrared quantum dots is the same as that of Example 1, except that after the injection of the selenium disulfide solution is completed, the reaction is continued for 10 minutes before the reaction is stopped.
[0090] Embodiment 3-4
[0091] A method for preparing uniform long-wave infrared quantum dots, as shown in Table 1, embodiments 3-4 are the same as embodiment 2, and the dropping speed of the selenium disulfide solution is limited to be the same, and the main difference lies in the concentration of the selenium disulfide solution and the injection volume of the selenium disulfide solution.
[0092] Table 1. Reference table of differences between Examples 3-4 and Example 2
[0093] <![CDATA[Concentration of SeS2 solution]]> <![CDATA[Volume of SeS2 solution injected]]> Example 3 0.04mol / L 7.5ml Example 4 0.025mol / L 12ml
[0094] Embodiment 5-7
[0095] A method for preparing uniform long-wave infrared quantum dots, as shown in Table 2, Examples 5-7 are the same as Example 1, and the dropping speed of the selenium disulfide solution is limited to the same, and the main difference is that the injection volume of the selenium disulfide solution is different, that is, the injection time is different.
[0096] Table 2. Reference table of differences between Examples 5-7 and Example 1
[0097] Example 5 Example 6 Example 7 Injection time 25min 30min 40min
[0098] Example 8
[0099] A method for preparing uniform long-wave infrared quantum dots is the same as that of Example 2, except that the reaction temperature during the nucleation and growth process is 120°C.
[0100] Comparative Example 1
[0101] A method for preparing quantum dots is the same as that in Example 2, and the dropping speed of the selenium disulfide solution is the same, and the main difference is that the concentration of the selenium disulfide solution is 0.005 mol / L and the injection volume of the selenium disulfide solution is 60 ml.
[0102] Comparative Example 2
[0103] A method for preparing quantum dots is the same as that of Example 2, except that the injection speed of the selenium disulfide solution is 0.03 ml / min.
[0104] Comparative Example 3
[0105] A method for preparing quantum dots is the same as that in Example 1, and the dropping speed of the selenium disulfide solution is limited to be the same, and the main difference is that the injection time of the selenium disulfide solution is 10 minutes.
[0106] Comparative Example 4
[0107] A method for preparing quantum dots is the same as that in Example 1, and the dropping speed of the selenium disulfide solution is limited to be the same, and the main difference is that the injection time of the selenium disulfide solution is 50 minutes.
[0108] Comparative Example 5
[0109] A method for preparing quantum dots is the same as that of Example 2, except that step 2 and step 3 are not included, and in step 4, a selenium disulfide solution is directly injected into a mercury precursor solution.
[0110] Comparative Example 6
[0111] A method for preparing quantum dots comprises the following steps:
[0112] Step 1, same as step 1 in Example 2;
[0113] Step 2: Prepare a 0.5 mol / L selenium disulfide solution. Specifically, weigh 143 mg (1 mmol) of selenium disulfide precursor as a Se source and dissolve it in 2 ml of OLA to obtain a selenium disulfide solution. The dissolution temperature is 140° C. and the reaction time is 1 h.
[0114] Step 3, nucleation: 0.25 ml of selenium disulfide solution was rapidly injected into the mercury precursor solution at 130° C. and reacted for 3 minutes to obtain a first solution;
[0115] Steps 4-6 are the same as steps 4-6 in Example 2.
[0116] Comparative Example 7
[0117] A method for preparing quantum dots comprises the following steps:
[0118] Steps 1 to 3 are the same as steps 1 to 3 in Example 2;
[0119] Step 4: prepare a 0.05 mol / L selenourea solution. Specifically, weigh 123 mg (1 mmol) of selenourea precursor as a Se source and dissolve it in 20 ml of OLA to obtain a selenourea solution. The dissolution temperature is 220° C. and the dissolution time is 2 h.
[0120] Step 5, growth: draw 8 ml of selenourea solution with a 10 ml syringe, place the syringe on a syringe pump, set the injection rate to 0.3 ml / min and inject the selenourea solution into the first solution at 130° C. for 20 min (a total of 6 ml of selenium disulfide solution is injected), continue the reaction for 10 min after the injection is completed, and then inject 12 ml of tetrachloroethylene (TCE) into the reaction solution as a cooling liquid to stop the reaction, thereby obtaining a second solution;
[0121] Step 6: Same as step 6 in Example 2.
[0122] Comparative Example 8
[0123] A method for preparing quantum dots comprises the following steps:
[0124] Step 1, same as step 1 in Example 2;
[0125] Step 2-3, same as step 2-3 of comparative example 6;
[0126] Steps 4-5, same as steps 4-5 of comparative example 7;
[0127] Step 6: Same as step 6 in Example 2.
[0128] test
[0129] 1. Fourier transform infrared spectroscopy test
[0130] Test method: Take 1 ml of the prepared quantum dot solution and centrifuge it (ethanol), then disperse it with TCE to obtain a dispersed quantum dot solution, drop the dispersed quantum dot solution on the ZnSe window, treat it with a gelator, soak it in 1,2-ethanedithiol (EDT), and then wash it twice with ethanol to obtain a sample to be tested; the sample to be tested is tested with a Fourier transform infrared spectrometer.
[0131] The quantum dots obtained from Examples 1-8, Comparative Examples 1-4, and Comparative Examples 6-8 were tested by Fourier transform infrared spectroscopy. The test results are as follows: Figure 1-13 As shown in the figure, the horizontal axis of the Fourier infrared absorption spectrum is the wave number (Wavenumber (cm -1 )), where wave number (cm -1 )=10000 / wavelength(μm), the ordinate is absorbance(au), that is, the absorption intensity. Some figures have been normalized, so the absorption intensity is not discussed here.
[0132] 2. TEM and particle size distribution test
[0133] TEM testing method: Put the copper mesh film in a white disc, wash the prepared quantum dots, disperse them with TCE to obtain a dispersed quantum dot solution, drop the dispersed quantum dot solution onto the copper mesh to obtain a sample to be tested; the sample to be tested is tested with a scanning electron microscope.
[0134] Particle size distribution test method: Based on the obtained TEM images, Nano Measuer software was used to perform particle size statistics.
[0135] The quantum dots obtained in Example 1, Example 2, Example 6, and Comparative Examples 4-8 were subjected to TEM and particle size distribution tests. The test results are as follows: Figure 14-21 shown.
[0136] 3. Data Analysis
[0137] According to the quantum confinement effect, when the size of a nanoparticle is smaller than its exciton Bohr radius, the smaller the particle size, the larger the band gap; on the contrary, the larger the particle size, the smaller the band gap, the longer the wavelength of the very long wave, the lower the energy, and this energy can only be absorbed by quantum dots with narrow band gaps. To reach the long-wave band, the size of the quantum dot material needs to be increased to meet the light absorption requirements. Furthermore, the poor uniformity of the size and morphology of the quantum dot material has a great impact on the performance of the subsequent device, so it is necessary to increase the uniformity of the size and morphology of the quantum dot.
[0138] 3.1. About Example 1
[0139] Figure 2 The Fourier transform infrared absorption spectrum of the long-wave infrared quantum dots prepared in Example 1 is as follows: Figure 2 It can be seen that its absorption peak is 7.55μm, which is basically close to the long-wave infrared band, and the absorption coverage range extends to the long-wave band and even the very long-wave band;
[0140] Fig.14 (a), 14(b), and 14(c) are TEM images of the long-wave infrared quantum dots prepared in Example 1 at different resolutions. Fig.14 (a), 14(b), and 14(c), it can be seen that the quantum dots are spherical in shape and have good uniformity in size and morphology;
[0141] Fig.14 (d) is the particle size distribution diagram of the long-wave infrared quantum dots prepared in Example 1. It can be seen from the figure that the average size of the quantum dots is d=16.76±4.05nm, further indicating that the size and morphology are uniform.
[0142] 3.2. Regarding Example 2 (Effect of Ripening on Quantum Dot Growth)
[0143] Figure 3 The Fourier transform infrared absorption spectrum of the long-wave infrared quantum dots prepared in Example 2 is as follows: Figure 3 It can be seen that its absorption peak is 8.84 μm, covering a range of 7-15 μm, and the absorption wavelength is red-shifted relative to Example 1, indicating that the size of the quantum dots has become larger, which can be further verified by the subsequent particle size distribution diagram;
[0144] Fig.15 (a), 15(b), and 15(c) are TEM images of the long-wave infrared quantum dots prepared in Example 2 at different resolutions. Fig.15 (a), 15(b), and 15(c) show that the size and morphology of the quantum dots are uniform and better than the quantum dots prepared in Example 1;
[0145] Fig.15 (d) is the particle size distribution diagram of the long-wave infrared quantum dots prepared in Example 2. It can be seen from the figure that the average size of the quantum dots is d=17.34±0.44nm, and its variance 0.44 is smaller than 4.05 in Example 1, which further illustrates that the size and morphology uniformity of the long-wave infrared quantum dots prepared in Example 2 are better than those in Example 1. The main reason is that after the injection of the selenium disulfide solution is completed, the embodiment continues the aging reaction for 10 minutes after the injection of the selenium disulfide solution is completed, and during this reaction time period, the small-sized quantum dots are more inclined to dissolve, while the large-sized quantum dots are more inclined to grow, so that the quantum dots are more uniform in size and morphology under the condition of increasing the size to meet the size requirements of the long-wave infrared.
[0146] 3.3. About Examples 3, 4 and Comparative Example 1 (Effect of Injected Selenium Disulfide Concentration on Quantum Dot Growth)
[0147] The difference between Example 3, Example 4 and Comparative Example 1 and Example 2 is that the amount of selenium disulfide relative to the mercury source is the same, but the solution concentration is lowered, and the dropwise reaction time is increased under the same injection speed. Specifically:
[0148] Figure 4 (a) Figure 4 (b) are the Fourier transform infrared absorption spectra of the long-wave infrared quantum dots prepared in Examples 3 and 4, respectively. Figure 4 (a) Figure 4 (b) with Figure 3 By comparison, it can be seen that as the concentration of selenium disulfide decreases and the addition time is extended, the absorption peaks red-shift from Example 2 (8.84 μm) to Example 3 ( Figure 4 (a)) 9.22 μm, Example 4 ( Figure 4 (b)) is 10.36 μm, that is, under the condition of ensuring a certain total amount, the selenium disulfide concentration is reduced and the injection time is extended, which can increase the size of long-wave infrared quantum dots;
[0149] Figure 7 The Fourier infrared absorption spectrum of the long-wave infrared quantum dots prepared in Comparative Example 1 is shown in FIG. Figure 7 It can be seen that as the concentration of selenium disulfide further decreases, the concentration required for quantum dot growth will not be reached, and the added SeS2 cannot be used for growth.
[0150] 3.4. About Examples 5, 6, 7 and Comparative Examples 3 and 4 (Effect of the Amount of Injected Selenium Disulfide on the Growth of Quantum Dots)
[0151] The difference between Comparative Example 3, Example 5, Example 6, Example 7 and Comparative Example 4 and Example 1 is that the injection time of selenium disulfide is different under the condition of the same injection speed, wherein Example 1 is injected for 20 minutes, while Comparative Example 3, Example 5, Example 6, Example 7 and Comparative Example 4 are injected for 10 minutes, 25 minutes, 30 minutes, 40 minutes and 50 minutes respectively;
[0152] Fig. 9 , Figure 5 (a) Figure 5 (b) Figure 5 (c) Fig.10 The Fourier infrared absorption spectra of the long-wave infrared quantum dots prepared in Comparative Example 3, Example 5, Example 6, Example 7, and Comparative Example 4 correspond to each other,
[0153] according to Fig. 9 , Figure 5 (a) Figure 5 (b) Figure 5 (c) Fig.10 as well as Figure 2 By comparison, as the injection time increases from 10 min to 50 min, the absorption peaks of the absorption spectrum are 6.83 μm, 7.55 μm, 8.6 μm, 9.02 μm, 9.42 μm, and 10.37 μm, respectively, that is, the absorption spectrum is red-shifted, and the size of the quantum dots increases. However, as the amount of injected selenium disulfide increases, the dispersion of the quantum dots becomes worse. When the injection time increases to 50 min, obvious precipitation can be seen in the later stage of the reaction. When it further grows to 58 min, the precipitation intensifies. Specifically:
[0154] When the reaction time increases to 30 min, the absorption spectrum of the product is Figure 5 (b), TEM images of the unfiltered product at different resolutions are shown in Fig.16 (a), 16(b), 16(c), the particle size distribution of the product is shown in Fig.16 (d) It can be seen that the average size of the quantum dots is 22.93 nm, the size has increased, and the size and morphology are uniform, but weaker than the product in Example 1;
[0155] When the reaction time increases to 50 min, the absorption spectrum shows Fig.10 TEM images of the product at different resolutions are shown in Fig.17 (a), 17(b), 17(c), and the particle size distribution diagram is shown in Fig.17 (d) Compared with the relevant test results of HgSe quantum dots obtained in Example 1, it can be seen that although the size is significantly increased, the uniformity is poor.
[0156] 3.5. Regarding Example 8 (different reaction temperatures)
[0157] The difference between Example 8 and Example 2 is that the reaction temperature is 120°C. Among the products obtained by the reaction, the quantum dots of the upper solution, the solid-liquid blend, and the lower precipitation have different sizes and absorption wavelengths. The quantum dots of the lower precipitation are larger and have a longer wavelength. Figure 6 The Fourier transform infrared absorption spectrum of the long-wave infrared quantum dots (lower layer precipitation) prepared in Example 8 is as follows: Figure 6 It can be seen that the absorption peak is 11.3 μm, which is significantly red-shifted compared to Example 2, indicating that the size of the quantum dots has increased and the uniformity is weaker than that of Example 2.
[0158] 3.6. Comparative Example 2 (different injection speeds)
[0159] The difference between Comparative Example 2 and Example 2 is that the injection rate of the selenium disulfide solution is changed to 0.03 ml / min. Figure 8 The Fourier infrared absorption spectrum of the long-wave infrared quantum dots prepared in Comparative Example 2 is shown in FIG. Figure 8 It can be seen that the absorption peak is 9.42 μm, which is significantly red-shifted compared to Example 2, indicating that the quantum dot size has become larger, but the main reason is that the reaction time is extended and the uniformity is weaker than that of Example 2.
[0160] 3.7. Comparative Example 5 (excluding nucleation operation)
[0161] The difference between Comparative Example 5 and Example 2 is that the nucleation operation is not included. Fig.18 TEM image of the long-wave infrared quantum dots prepared in Comparative Example 5. Fig.18 It can be seen that the morphology and size of quantum dots are highly non-uniform.
[0162] 3.8. Comparative Example 6 (Replacing the Nucleation Selenourea Solution with Selenium Disulfide Solution)
[0163] The difference between Comparative Example 6 and Example 2 is that the nucleation selenium source is replaced by selenium disulfide from selenourea. Fig.11 The Fourier transform infrared absorption spectra of the long-wave infrared quantum dots prepared in Comparative Example 6 under unfiltered and filtered conditions are shown in Table 1. Fig.11 It can be seen that its dispersion is poor and the quantum dots are agglomerated. For details, see the TEM of the unfiltered product. Fig.19 (a) TEM of filtration products Fig.19 (b), it can be seen that the uniformity of the HgSe quantum dots obtained is poor compared to that obtained in Example 2;
[0164] During the above experiment, 0.5 mol / L selenium disulfide solution could not be completely dissolved. The concentration of selenium disulfide solution used for nucleation was further adjusted to 0.25 mol / L by gradient. It was found that the uniformity of size and morphology was still weaker than that of the product obtained in Example 2.
[0165] 3.8. Comparative Example 7 (Replacing the Growth Selenium Disulfide Solution with Selenourea Solution)
[0166] The difference between Comparative Example 7 and Example 2 is that the selenium source for growth is replaced by selenium urea instead of selenium disulfide. Fig.12 The Fourier infrared absorption spectrum of the long-wave infrared quantum dots prepared in Comparative Example 6 is shown in Table 1. Fig.12 It can be seen that the quantum dot detection wavelength is shorter than that of the product in Example 2, and almost does not reach the long-wave range; further, the TEM images of the product at different resolutions are as follows: Fig. 20 (a), 20(b), and 20(c), and the particle size distribution diagram is shown in Fig. 20 (d) as shown, according to Fig. 20 It can be seen that the uniformity of its size and morphology is poor.
[0167] 3.9. Comparative Example 8 (replacing the nucleation selenourea solution with a selenium disulfide solution, and the growth selenium disulfide solution with a selenourea solution)
[0168] The difference between Comparative Example 8 and Example 2 is that the nucleation selenourea solution is replaced by a selenium disulfide solution, and the growth selenium disulfide solution is replaced by a selenourea solution. Fig.13 The Fourier infrared absorption spectrum of the long-wave infrared quantum dots prepared in Comparative Example 8 is shown in FIG. Fig.13 It can be seen that the quantum dot detection wavelength is shorter than that of the product in Example 2, and almost does not reach the long-wave range; further, the TEM images of the product at different resolutions are as follows: Fig.21 (a), 21(b), and 21(c), and the particle size distribution diagram is shown in Fig.21 (d) as shown, according to Fig. 20 It can be seen that the uniformity of its size and morphology is poor.
[0169] The embodiments of this specific implementation are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. The same components are represented by the same figure marks. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing uniform long-wave infrared quantum dots, characterized in that: The following steps are involved: Prepare 0.07-0.1 mol / L mercury precursor solution; Prepare 0.4-0.6 mol / L selenourea solution, inject mercury precursor solution, react at 120-150° C. for 2-10 min to obtain a first solution, wherein the volume ratio of selenourea solution to mercury precursor solution is 1:20-30; A 0.025-0.06 mol / L selenium disulfide solution is prepared, and the selenium disulfide solution is uniformly injected into the first solution at 120-150° C., and the injection time is controlled to be 15-40 min to obtain a second solution, wherein the volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:0.5-1.2; The second solution is purified to obtain uniform long-wave infrared quantum dots.
2. The method for preparing uniform long-wave infrared quantum dots according to claim 1, characterized in that: The concentration of the mercury precursor solution is 0.075-0.09 mol / L, the concentration of the selenourea solution is 0.45-0.55 mol / L, and the volume ratio of the selenourea solution to the mercury precursor solution is 1:22-26.
3. The method for preparing uniform long-wave infrared quantum dots according to claim 2, characterized in that: The concentration of the mercury precursor solution is 0.083 mol / L, the concentration of the selenourea solution is 0.5 mol / L, and the volume ratio of the selenourea solution to the mercury precursor solution is 1:
24.
4. The method for preparing uniform long-wave infrared quantum dots according to claim 1, characterized in that: The reaction time of the selenourea solution and the mercury precursor solution is 2.5-3.5 min.
5. The method for preparing uniform long-wave infrared quantum dots according to claim 1, characterized in that: The reaction temperature is 128-132°C.
6. The method for preparing uniform long-wave infrared quantum dots according to claim 1, characterized in that: A 0.045-0.055 mol / L selenium disulfide solution is prepared, and the selenium disulfide solution is uniformly injected into the first solution while controlling the injection time to be 18-22 minutes. The volume ratio of the selenium disulfide solution to the mercury precursor solution is 1:0.8-1.
2.
7. The method for preparing uniform long-wave infrared quantum dots according to claim 6, characterized in that: A 0.05 mol / L selenium disulfide solution was prepared, and the selenium disulfide solution was uniformly injected into the first solution while controlling the injection time to be 20 min. The volume ratio of the selenium disulfide solution to the mercury precursor solution was 1:
1.
8. The method for preparing uniform long-wave infrared quantum dots according to claim 1, characterized in that: After the injection is completed, the reaction continues for 8-12 minutes.
9. Uniform long-wave infrared quantum dots, characterized in that: The uniform long-wave infrared quantum dots are prepared by the preparation method according to any one of claims 1 to 8.
10. A photodetector, characterized in that Comprising the uniform long-wave infrared quantum dots as described in claim 9.