Soil stabilizer for road surface layer and preparation method of soil stabilizer
Through soil curing agents composed of sodium silicate, polyacrylamide, etc., the problems of low compressive strength and difficult water content control of the road surface layer are solved, high compressive strength and stability are achieved, and the service life of the road is extended.
Patent Information
- Application Number
- CN202411308960.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing soil curing agent is used in the road surface layer with low compressive strength, which is difficult to withstand heavy vehicles and harsh climate, resulting in cracks and damage on the road surface layer, and it is difficult to control the soil moisture content during construction, affecting the leveling of the road. degree and stability.
Soil curing agent composed of sodium silicate, polyacrylamide, ethylene glycol, silane coupling agent, nanomontmorillonite and defoaming agent are used to form a soil curing agent with high compressive strength and stability through specific proportions and processes. Liquid soil curing agent, adjusts the moisture content of the soil to improve the durability of the road.
It significantly improves the compressive strength of the road surface layer, reduces the expansion and contraction caused by moisture changes, extends the service life of the road, and ensures stability and reliability under different climatic conditions.
Smart Images

Figure BDA0005050089040000071 
Figure BDA0005050089040000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of soil solidifiers, and in particular relates to a soil solidifier for a road surface layer and a preparation method thereof. Background Art
[0002] Soil stabilizer is a chemical agent used to enhance soil strength and stability, and is widely used in engineering projects such as road construction, foundation treatment, and dam reinforcement. Its working principle is mainly to change the microstructure of the soil through chemical reactions or physical effects, thereby significantly improving the physical and mechanical properties of the soil.
[0003] Specifically, soil stabilizers can improve the compressive and shear strengths of soil, making it more stable when subjected to external loads. This enhancement effect is mainly due to the interaction between the stabilizer and soil particles, which forms a tighter bond and reduces the gaps between soil particles, thereby improving the overall density and strength. In addition, stabilizers can also improve the durability of soil, resist erosion by environmental factors such as moisture and freeze-thaw cycles, and extend the service life of soil.
[0004] In practical applications, the selection and proportion of soil stabilizers are crucial. Different types of stabilizers, such as sodium silicate and polyacrylamide, have different chemical properties and reaction mechanisms, and can be optimized for specific soil types and engineering requirements. Through reasonable proportioning and use, soil stabilizers can not only improve the bearing capacity of the soil, but also effectively reduce the maintenance cost of the project and improve the overall economic benefits of the project.
[0005] However, the existing soil solidifiers are mainly used for road bases, and the compressive strength of the surface layer is generally low, which is difficult to withstand the impact of heavy vehicles and bad weather, resulting in cracks and damage on the road surface, affecting the service life of the road and driving safety. In addition, during the construction process, the existing soil solidifiers are often difficult to effectively control the moisture content of the soil, resulting in the solidified soil being easily swollen due to moisture or shrinking due to drying, affecting the flatness and stability of the road.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, provide a soil solidifying agent for road surface and a preparation method, and solve the problems raised in the above background technology.
[0008] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:
[0009] A soil solidifying agent for road surface and a preparation method thereof, comprising: the following components in weight percentage range: 3-5% sodium silicate, 1-2% polyacrylamide, 0.5-1.5% ethylene glycol, 0.5-1.0% silane coupling agent, 0.2-0.5% titanium dioxide, 0.1-0.3% nano-montmorillonite, 0.01-0.1% defoaming agent, an appropriate amount of pH regulator to maintain the pH value between 7 and 9, and the balance being water.
[0010] Sodium silicate is the main curing agent, providing a silicon-oxygen chain structure to enhance the strength and stability of the soil. Polyacrylamide, as a thickener and binder, can improve the adhesion of the mixture and improve the bonding between soil particles. The combination of polyacrylamide and water improves the fluidity of the mixture and promotes the uniform distribution of other ingredients. Sodium silicate reacts with water to form silicates, which enhances the curing effect of the soil. Silane coupling agents enhance the bonding between the curing agent and soil particles through chemical bonding, improving the overall strength. The introduction of nano-montmorillonite improves the microstructure of the material and improves its compression and crack resistance.
[0011] Optionally, the sodium silicate is a solid powder.
[0012] Optionally, the polyacrylamide solid powder has a particle size of 10-50 μm and a molecular weight of 122.06 g / mol.
[0013] Optionally, ethylene glycol is in liquid state, has a molecular weight of 62.07 g / mol, and a viscosity of 16.1 mPas.
[0014] Optionally, titanium dioxide is solid powder with a molecular weight of 79.87 g / mol and a particle size of 20-30 nm.
[0015] Optionally, the nano-montmorillonite is solid powder with a particle size of 10 nm.
[0016] A method for preparing a soil solidifying agent for a road surface layer comprises the following steps:
[0017] Step (1): adding water into a reaction kettle and heating the water to 60° using steam, then starting a stirring device, and then adding sodium silicate, polyacrylamide, and ethylene glycol into the stirring device and stirring until uniformly mixed to obtain product ①;
[0018] Step (2): adding silane coupling agent, titanium dioxide and nano-montmorillonite to the product ① in sequence during stirring, and mixing evenly to obtain the product ②;
[0019] Step (3): Add a defoaming agent to the product ② during stirring and mix well to obtain the product ③;
[0020] Step (4): during the stirring process, a pH regulator is added to the product ③ to maintain the pH value of the curing agent between 7 and 9;
[0021] Step (5): After all the raw materials are completely dissolved, continue stirring for 1-3 hours to obtain the soil solidifying agent;
[0022] Step (6): Use a filter to filter the solids from the soil stabilizer, put the filtered liquid into a bucket, attach a label and keep the sample sealed.
[0023] Optionally, the pores in the filter are 300 mesh.
[0024] Optionally, the stirring speed during the stirring process is 500 rpm.
[0025] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art. Of course, any product implementing the present invention does not necessarily need to achieve all the advantages described below at the same time:
[0026] After the liquid soil solidifier of the present invention is mixed with soil, it can significantly improve the compressive strength of the road surface layer, and the 7-day compressive strength can reach more than 4.6 MPa, effectively reducing the problem of surface cracking. This significantly improved compressive strength is mainly due to the interaction between the chemical components contained in the solidifier and the soil particles, forming a tighter structure and enhancing the overall stability of the soil. In addition, the use of the solidifier can effectively fill the gaps between soil particles, reduce the penetration and loss of water, and thus reduce the expansion and contraction of the soil caused by water changes.
[0027] Secondly, the liquid soil solidifying agent of the present invention can adjust and control the moisture content of the soil, so that the solidified soil has better drying performance and stability. By adjusting the moisture content of the soil, the solidifying agent can effectively reduce the negative impact of excessive moisture in the soil on the road quality and prevent the softening and strength loss of the soil caused by excessive moisture. This ability to control moisture not only improves the durability of the soil, but also extends the service life of the road, ensuring the stability and reliability of the soil structure under different climatic conditions.
[0028] The specific embodiments of the present invention are described in further detail below. DETAILED DESCRIPTION
[0029] The present invention will now be described in further detail.
[0030] A soil solidifying agent for a road surface layer comprises the following components in weight percentage range: 3-5% sodium silicate, 1-2% polyacrylamide, 0.5-1.5% ethylene glycol, 0.5-1.0% silane coupling agent, 0.2-0.5% titanium dioxide, 0.1-0.3% nano-montmorillonite, 0.01-0.1% defoaming agent, an appropriate amount of pH regulator to maintain the pH value between 7 and 9, and the balance is water.
[0031] In this embodiment, the sodium silicate is a solid powder.
[0032] In this embodiment, the polyacrylamide solid powder has a particle size of 10-50 μm and a molecular weight of 122.06 g / mol.
[0033] In this embodiment, ethylene glycol is in liquid state, has a molecular weight of 62.07 g / mol, and a viscosity of 16.1 mPas.
[0034] In this embodiment, titanium dioxide is solid powder with a molecular weight of 79.87 g / mol and a particle size of 20-30 nm.
[0035] In this embodiment, the nano-montmorillonite is solid powder with a particle size of 1-10 nm.
[0036] A method for preparing a soil solidifying agent for a road surface layer comprises the following steps:
[0037] Step (1): adding water into a reaction kettle and heating the water to 60° using steam, then starting a stirring device, and then adding sodium silicate, polyacrylamide, and ethylene glycol into the stirring device and stirring until uniformly mixed to obtain product ①;
[0038] Step (2): adding silane coupling agent, titanium dioxide and nano-montmorillonite to the product ① in sequence during stirring, and mixing evenly to obtain the product ②;
[0039] Step (3): Add a defoaming agent to the product ② during stirring and mix well to obtain the product ③;
[0040] Step (4): during the stirring process, a pH regulator is added to the product ③ to maintain the pH value of the curing agent between 7 and 9;
[0041] Step (5): After all the raw materials are completely dissolved, continue stirring for 1-3 hours to obtain the soil solidifying agent;
[0042] Step (6): Use a filter to filter the solids from the soil stabilizer, put the filtered liquid into a bucket, attach a label and keep the sample sealed.
[0043] In this embodiment, the filter pores in the filter are 100-300 meshes.
[0044] In this embodiment, the stirring speed during the stirring process is 300-500 rpm.
[0045] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0046] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0047] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0048] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0049] In the following examples, "ratio" means the proportion of a certain raw material component in the total mass of the raw materials.
[0050] It should be noted that all raw materials used in the examples of the present invention were obtained through commercial channels.
[0051] Example 1: In this example, a soil solidifier for a road surface is provided, comprising the following components in the following weight percentage ranges: sodium silicate: 4%, polyacrylamide: 1.5%, ethylene glycol: 1%, silane coupling agent: 0.7%, titanium dioxide: 0.3%, nano-montmorillonite: 0.2%, defoaming agent: 0.05%, the remainder being water, and an appropriate amount of pH regulator to maintain a pH value between 7.
[0052] Example 2: In this example, a soil solidifier for a road surface is provided, comprising the following components in the following weight percentage ranges: sodium silicate: 3.5%, polyacrylamide: 1.8%, ethylene glycol: 1.2%, silane coupling agent: 0.6%, titanium dioxide: 0.4%, nano-montmorillonite: 0.15%, defoaming agent: 0.08%, the remainder being water, and an appropriate amount of pH regulator to maintain the pH value between 7.
[0053] Example 3: In this example, a soil solidifier for a road surface is provided, comprising the following components in the following weight percentage ranges: sodium silicate: 5%, polyacrylamide: 2%, ethylene glycol: 1.5%, silane coupling agent: 1%, titanium dioxide: 0.5%, nano-montmorillonite: 0.3%, defoaming agent: 0.1%, the balance being water, and an appropriate amount of pH regulator to maintain the pH value between 7.
[0054] Example 4: In this example, a soil solidifier for road surface is provided, comprising the following components in the following weight percentage ranges: sodium silicate: 3%, polyacrylamide: 1%, ethylene glycol: 0.5%, silane coupling agent: 0.5%, titanium dioxide: 0.2%, nano-montmorillonite: 0.1%, defoaming agent: 0.01%, the balance being water, and an appropriate amount of pH regulator to maintain the pH value between 7.
[0055] Experimental Example 1: Bond Strength (kPa) Test
[0056] First, mix the liquid soil solidifier and standard soil in a weight ratio of 1:4 to ensure uniform mixing. Use a standard test mold and apply a thin layer of release agent on the inner surface of the mold to prevent the mixture of the solidifier and soil from adhering to the mold. Pour the mixed soil solidifier into the test mold, and be careful to prevent bubbles from forming during the pouring process. Use a vibration table to gently vibrate the test mold so that the mixture of the solidifier and soil fully fills the mold and removes bubbles. After the solidifier and soil mixture is cured at room temperature for 24 hours, remove the mold and test it using a bond strength tester. Place the specimen on the support platform of the tester, ensuring that the specimen is parallel to the tester probe. Apply tension at a uniform speed until the specimen breaks, record the maximum destructive force, and obtain the experimental results as shown in Table 1.
[0057]
[0058]
[0059] The experimental results show that sodium silicate can react with minerals in the soil to form silicate gel, which enhances the structural stability of the soil. It can improve the adhesion between soil particles and improve the overall strength of the soil. Ethylene glycol can improve the fluidity and dispersibility of the curing agent and promote the uniform mixing of other ingredients, thereby improving the bonding effect. Silane coupling agent can enhance the interfacial bonding between soil and curing agent, improve the resistance to moisture and chemicals, and further improve the bonding strength. Titanium oxide can increase the compressive strength of the soil and improve the durability of the soil through its photocatalytic properties. The high specific surface area and layered structure of nano-montmorillonite can effectively fill the gaps between soil particles and enhance the overall strength and stability of the soil.
[0060] Furthermore, the addition of liquid soil stabilizer significantly improved the tensile strength of the soil. Specifically, the soil samples that had been stabilized showed higher strength values in the maximum destructive force test, indicating that the stabilizer formed a stronger bond between soil particles. This phenomenon can be attributed to the chemical cross-linking structure formed by the stabilizer in the soil, which effectively enhanced the overall stability of the soil.
[0061] The present invention is not limited to the above-mentioned embodiments. Anyone should be aware that any structural changes made under the enlightenment of the present invention, and any technical solutions that are the same or similar to the present invention, fall within the protection scope of the present invention. The technology, shape, and structural parts not described in detail in the present invention are all well-known technologies.
Claims
1. A soil solidifying agent for road surface, characterized in that: The components are in the following weight percentage range: 3-5% sodium silicate, 1-2% polyacrylamide, 0.5-1.5% ethylene glycol, 0.5-1.0% silane coupling agent, 0.2-0.5% titanium dioxide, 0.1-0.3% nano-montmorillonite, 0.01-0.1% defoaming agent, an appropriate amount of pH regulator to maintain the pH value between 7 and 9, and the balance is water.
2. The soil solidifying agent for road surface according to claim 1, characterized in that: Sodium silicate is a solid powder.
3. The soil solidifying agent for road surface according to claim 1, characterized in that: Polyacrylamide solid powder, particle size is 10-50μm, molecular weight is 122.06g / mol.
4. The soil solidifying agent for road surface according to claim 1, characterized in that: Ethylene glycol is in liquid state, with a molecular weight of 62.07 g / mol and a viscosity of 16.1 mPas.
5. The soil solidifying agent for road surface according to claim 1, characterized in that: Titanium dioxide is a solid powder with a molecular weight of 79.87 g / mol and a particle size of 20-30 nm.
6. The soil solidifying agent for road surface according to claim 1, characterized in that: Nano-montmorillonite is a solid powder with a particle size of 1-10nm.
7. The method for preparing a soil solidifying agent for road surface according to claim 1, characterized in that: The following steps are involved: Step (1): adding water into a reaction kettle and heating the water to 60° using steam, then starting a stirring device, and then adding sodium silicate, polyacrylamide, and ethylene glycol into the stirring device and stirring until uniformly mixed to obtain product ①; Step (2): adding silane coupling agent, titanium dioxide and nano-montmorillonite to the product ① in sequence during stirring, and mixing evenly to obtain the product ②; Step (3): Add a defoaming agent to the product ② during stirring and mix well to obtain the product ③; Step (4): during the stirring process, a pH regulator is added to the product ③ to maintain the pH value of the curing agent between 7 and 9; Step (5): After all the raw materials are completely dissolved, continue stirring for 1-3 hours to obtain the soil solidifying agent; Step (6): Use a filter to filter the solids from the soil stabilizer, put the filtered liquid into a bucket, attach a label and keep the sample sealed.
8. The method for preparing a soil solidifying agent for a road surface layer according to claim 1, characterized in that: The pores in the filter are 100-300 mesh.
9. The method for preparing a soil solidifying agent for a road surface layer according to claim 1, characterized in that: The stirring speed during the stirring process is 300-500 rpm.