Antioxidant high-temperature-resistant lubricating grease and preparation method thereof

By using chemical bonding of hindered phenol modified silicone oil to HPDMS silicone oil in grease and combining with other additives, the problems of unstable and poor antioxidant compatibility of traditional greases at high temperatures are solved, and the performance improvement of grease at high temperatures is achieved and food safety guarantee.

CN119060769APending Publication Date: 2024-12-03ANHUI BOYANG LUBRICATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185031.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional greases are unstable at high temperatures, tend to become thinner and lose adhesion, resulting in poor lubrication and equipment damage, and poor compatibility with the matrix and easy precipitation, affecting food safety.

Method used

Using hindered phenol modified silicone oil as the base oil, it is chemically bonded with HPDMS silicone oil, combined with extreme pressure anti-wear agent, corrosion agent and anti-mold agent to form antioxidant and high-temperature grease, and improve grease through specific synthesis methods and process treatments. Antioxidant and high temperature resistance.

Benefits of technology

It improves the antioxidant ability and high temperature stability of the grease, solves the problems of poor compatibility and easy precipitation of antioxidants, and ensures the performance stability and safety of the grease at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013265890000081
    Figure BDA0005013265890000081
Patent Text Reader

Abstract

The invention discloses antioxidant high-temperature-resistant lubricating grease and a preparation method thereof, and belongs to the technical field of lubricating grease, the antioxidant high-temperature-resistant lubricating grease comprises the following raw materials by weight: 70-80 parts of hindered phenol modified silicone oil, 10-30 parts of a thickening agent, 1-3 parts of an anti-wear reagent at extreme pressure, 1-3 parts of a corrosion inhibitor, and 2-8 parts of an anti-mildew agent. The raw materials are mixed and stirred in a kneading machine, discharged and ground to obtain the lubricating grease. According to the invention, hindered phenol groups are introduced to silicone oil molecular chain ends to obtain hindered phenol modified silicone oil, and the lubricating grease synthesized by taking the hindered phenol modified silicone oil as base oil has excellent high temperature resistance and oxidation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lubricating grease, and in particular relates to an antioxidant and high temperature resistant lubricating grease and a preparation method thereof. Background Art

[0002] Grease is an important component of industrial lubricants. Grease technology has been continuously developing since its birth, and has formed a series of rich varieties of lubricating products. In recent years, with the development of science and technology and industry, mechanical equipment has developed in the direction of large-scale, miniature, high-speed, heavy-load, vacuum, low temperature, ultra-high precision, automation and intelligence. People's demand for new high-performance lubricating products is also increasing. The development of high-performance grease products with long service life and reliable lubrication in special occasions has huge market prospects and economic benefits, and has become a research and development hotspot of the grease industry in various countries in the world. With the rapid development of the economy, many mechanical equipment work under high temperature and high pressure conditions. The lubrication of its parts can no longer meet the lubrication requirements with general grease.

[0003] The use of traditional grease is below 120℃, such as calcium-based grease, the use temperature is not higher than 60℃, and the use temperature of lithium-based grease is not higher than 120℃. Greases with a maximum use temperature exceeding 120℃ are generally called high-temperature greases, such as composite lithium-based grease, composite barium-based grease, composite aluminum-based grease, polyurea grease, bentonite grease, silicone grease, fluoroether grease, etc. The maximum use temperature limit of composite soap high-temperature grease generally does not exceed 200℃.

[0004] Patent ZL201410026925.3 reports a food-grade grease composition and a preparation method thereof, which uses base oil, benzoic acid, stearic acid and aluminum isopropylate trimer as thickeners, and adds silicone oil, calcium carbonate, antioxidants, and rust inhibitors as auxiliary materials to prepare a food-grade composite aluminum-based grease. However, this type of grease will become thinner, its adhesion will decrease, and it will separate and drip at high temperatures. The grease will easily fall off the equipment, which will not only cause poor lubrication and damage to the equipment, but may also contaminate food and cause food safety accidents.

[0005] Publication No. CN107325863A discloses an antioxidant grease that can achieve good antioxidant and anti-corrosion capabilities by adding various materials. However, in the preparation of the antioxidant grease in this patent, only a common and single antioxidant component currently available on the market is mixed with an existing conventional grease material, and the mixing method is also a conventional processing method. Therefore, although the actual finished product has a certain antioxidant function, the antioxidant has poor compatibility with the matrix and is easy to precipitate. Summary of the invention

[0006] In order to solve the problems of high temperature instability of grease and easy precipitation of antioxidants mentioned in the background technology, the present invention provides an antioxidant and high temperature resistant grease and a preparation method thereof.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] An antioxidant and high temperature resistant lubricating grease, comprising the following raw materials, by weight: 70-80 parts of hindered phenol modified silicone oil, 10-30 parts of thickener, 1-3 parts of extreme pressure anti-wear agent, 1-3 parts of anti-corrosion agent, and 2-8 parts of antifungal agent;

[0009] The hindered phenol modified silicone oil is prepared by the following method:

[0010] BBHP and HPDMS were added to a three-necked flask, heated to 80°C, Pt solution was added, the temperature was raised to 120°C and refluxed for 2h to obtain hindered phenol-modified silicone oil, wherein BBHP was terminally allylated hindered phenol and HPDMS was dihydrogen-terminated dimethyl polysiloxane.

[0011] Furthermore, the HPDMS is prepared by the following method:

[0012] Octamethylcyclotetrasiloxane, 1,1,3,3-tetramethyldisiloxane and acid clay were added into a three-necked flask, heated to 70°C, and continued to heat for 4 hours. The acid clay was filtered off to obtain HPDMS.

[0013] Further, the BBHP is prepared by the following method:

[0014] Under a nitrogen atmosphere, 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid and 3-butene-1-ol were dissolved in dichloromethane, stirred for 10 min, and then 4-dimethylaminopyridine was added, stirred for 10 min, and a dichloromethane solution containing N,N-dicyclohexylcarbodiimide was added. After the reaction was completed, the reaction solution was poured into water, filtered and evaporated to obtain a crude product. The crude product was separated by silica gel column chromatography, eluted with an eluent, and evaporated under reduced pressure at -0.2 MPa and 60°C for 2 h to obtain BBHP.

[0015] Furthermore, the thickener is a powdered urea-based thickener.

[0016] Furthermore, the extreme pressure anti-wear agent is a complex of dithiodithiazolone and dialkyl copper dithiophosphate, and the mass ratio of dithiodithiazolone to dialkyl copper dithiophosphate is 1:1.

[0017] Furthermore, the anti-corrosion agent is at least one of T551 benzotriazole derivatives, T706 benzotriazole, and T561 oxadiazole derivatives.

[0018] Furthermore, the antifungal agent is at least one of 10,10'-oxybisphenoxane arsenic and tetrabutylammonium chloride.

[0019] Furthermore, the mass ratio of octamethylcyclotetrasiloxane, 1,1,3,3-tetramethyldisiloxane and acid clay is 15-20:1.7-2.4:0.5-1.

[0020] Furthermore, the usage ratio of 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid, 3-butene-1-ol, 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide is 5.2-5.8g: 1-1.6g: 0.18-0.20g: 4.6-5.2g.

[0021] Furthermore, the dosage ratio of N,N-dicyclohexylcarbodiimide to dichloromethane in the dichloromethane solution containing N,N-dicyclohexylcarbodiimide is 4.6-5.2 g:10-20 mL.

[0022] Furthermore, the eluent is a mixture of ethyl acetate and cyclohexanone, and the mass ratio of ethyl acetate to cyclohexanone is 1:9.

[0023] Furthermore, the reduced pressure evaporation has a vacuum degree of -0.2 MPa, a temperature of 60°C, and a time of 2 hours.

[0024] Furthermore, the dosage ratio of chloroplatinic acid to anhydrous ethanol in the Pt solution is 0.4-0.6 g:10-20 mL, and the mass ratio of BBHP, HPDMS and chloroplatinic acid is 50:25:4-6.

[0025] A method for preparing an antioxidant and high temperature resistant lubricating grease comprises the following steps:

[0026] Put hindered phenol modified silicone oil, thickener, extreme pressure anti-wear agent, corrosion inhibitor and mildew inhibitor into a kneader, mix and stir for 2 hours at 60-90°C, with a stirring speed of 40-50r / min; after the low-temperature mixing treatment is completed, heat up to 160-190°C, stir for 2 hours under a vacuum degree of 570mmHg, with a stirring speed of 30-40r / min; discharge the material, grind it twice with a three-roll grinder to obtain an antioxidant and high temperature resistant grease.

[0027] Beneficial effects of the present invention:

[0028] The invention synthesizes HPDMS silicone oil by double hydrogen-terminated dimethylpolysiloxane, introduces hindered phenol groups into the molecular chain ends of the HPDMS silicone oil, obtains hindered phenol-modified silicone oil and further synthesizes lubricating grease. The hydroxyl groups on the hindered phenol are subject to a strong steric hindrance effect, and the hydrogen on the hindered phenol is extremely active, and is easy to fall off and combine with peroxy free radicals and the like generated by polymer rupture to obtain stable phenol oxygen free radicals, thereby preventing a series of free radical chain reactions and improving the anti-oxidation ability of the lubricating grease. The extremely high bond energy of the silicon-oxygen bond makes it difficult to break at high temperatures, thereby improving the anti-high temperature ability of the lubricating grease. In addition, the hindered phenol and the HPDMS silicone oil are combined together by chemical bonding, thereby solving the problem that the antioxidant in the physical mixing method has poor compatibility and is easy to precipitate in the matrix. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The acid clay in the following examples and comparative examples was purchased from Jinan Xuanhua Chemical Co., Ltd., and the thickener was purchased from Shenzhen Asec Lubricating Materials Co., Ltd., which is a powdered urea-based thickener with a model of DG-105.

[0031] Example 1

[0032] A method for preparing an antioxidant and high temperature resistant lubricating grease comprises the following steps:

[0033] The first step, synthesis of dihydrogen-terminated dimethyl polysiloxane:

[0034] 150 g of octamethylcyclotetrasiloxane, 17 g of 1,1,3,3-tetramethyldisiloxane and 5 g of acid clay were added to a 250 mL dry three-necked flask equipped with a thermometer, a stirrer and a condenser, heated to 70° C., continued heating for 4 h, and filtered off the catalyst acid clay to obtain HPDMS;

[0035] Step 2: Synthesis of terminally allylated hindered phenols:

[0036] Under a nitrogen atmosphere at 0°C, 52 g of 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid and 10 g of 3-butene-1-ol were dissolved in 800 mL of dichloromethane and stirred for 10 min. 1.8 g of 4-dimethylaminopyridine was added and stirred for 10 min. 46 g of N,N-dicyclohexylcarbodiimide was dissolved in 100 mL of dichloromethane solution and added to the reaction system. After the reaction was completed, the reaction solution was poured into water, filtered and evaporated to obtain a crude product. The crude product was separated by silica gel column chromatography, eluted with an eluent consisting of 10 g of ethyl acetate and 90 g of cyclohexanone, and evaporated under reduced pressure at -0.2 MPa and 60°C for 2 h to obtain BBHP.

[0037] Step 3: Synthesis of hindered phenol modified silicone oil:

[0038] 50 g BBHP and 25 g HPDMS were added to a 250 mL dry three-necked flask equipped with a mixture meter, a stirrer and a condenser, and heated to 80 ° C. 4 g chloroplatinic acid was dissolved in 100 mL anhydrous ethanol and added to the three-necked flask. The solution temperature was raised to 120 ° C, bubbles were generated, and refluxed for 2 h to obtain hindered phenol-modified silicone oil.

[0039] Step 4: Synthesis of grease:

[0040] 35g of hindered phenol-modified silicone oil, 5g of thickener, 0.25g of dithiodithiazolone, 0.25g of dialkyl dithiophosphate copper, 0.5g of T551 benzotriazole derivative, and 1g of 10,10'-oxybisphenoxane were put into a kneader, and low-temperature mixing and stirring were carried out at 60°C for 2h, with a stirring speed of 40r / min; after the low-temperature mixing treatment was completed, the temperature was raised to 160°C, and stirred for 2h under a vacuum degree of 570mmHg, with a stirring speed of 30r / min; the material was discharged and ground twice on a three-roll grinder to obtain grease.

[0041] Example 2

[0042] A method for preparing an antioxidant and high temperature resistant lubricating grease comprises the following steps:

[0043] The first step, synthesis of dihydrogen-terminated dimethyl polysiloxane:

[0044] 180 g of octamethylcyclotetrasiloxane, 21 g of 1,1,3,3-tetramethyldisiloxane and 7 g of acid clay were added to a 500 mL dry three-necked flask equipped with a thermometer, a stirrer and a condenser, heated to 70° C., continued heating for 4 h, and filtered to remove the catalyst acid clay to obtain HPDMS;

[0045] Step 2: Synthesis of terminally allylated hindered phenols:

[0046] Under a nitrogen atmosphere at 0°C, 55 g of 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid and 13 g of 3-butene-1-ol were dissolved in 850 mL of dichloromethane and stirred for 10 min, and then 1.9 g of 4-dimethylaminopyridine was added and stirred for 10 min. 49 g of N,N-dicyclohexylcarbodiimide was dissolved in 150 mL of dichloromethane solution and added to the reaction system. After the reaction was completed, the reaction solution was poured into water, filtered and evaporated to obtain a crude product. The crude product was separated by silica gel column chromatography, eluted with an eluent consisting of 10 g of ethyl acetate and 90 g of cyclohexanone, and evaporated under reduced pressure at -0.2 MPa and 60°C for 2 h to obtain BBHP;

[0047] Step 3: Synthesis of hindered phenol modified silicone oil:

[0048] 50 g BBHP and 25 g HPDMS were added to a 250 mL dry three-necked flask equipped with a mixture meter, a stirrer and a condenser, and heated to 80 ° C. 5 g chloroplatinic acid was dissolved in 150 mL anhydrous ethanol and added to the three-necked flask. The solution temperature was raised to 120 ° C, bubbles were generated, and refluxed for 2 hours to obtain hindered phenol-modified silicone oil.

[0049] Step 4: Synthesis of grease:

[0050] 37g of hindered phenol modified silicone oil, 10g of thickener, 0.5g of dithiodithiazolone, 0.5g of dialkyl dithiophosphate copper, 1g of T706 benzotriazole and 2.5g of tetrabutylammonium chloride were put into a kneader and mixed and stirred at low temperature for 2h at 75°C with a stirring speed of 45r / min; after the low temperature mixing treatment was completed, the temperature was raised to 175°C, and stirred for 2h at a vacuum degree of 570mmHg with a stirring speed of 35r / min; the material was discharged and ground twice on a three-roll grinder to obtain grease.

[0051] Example 3

[0052] A method for preparing an antioxidant and high temperature resistant lubricating grease comprises the following steps:

[0053] The first step, synthesis of dihydrogen-terminated dimethyl polysiloxane:

[0054] 200 g of octamethylcyclotetrasiloxane, 24 g of 1,1,3,3-tetramethyldisiloxane and 10 g of acid clay were added to a 500 mL dry three-necked flask equipped with a thermometer, a stirrer and a condenser, heated to 70° C., continued heating for 4 h, and filtered off the catalyst acid clay to obtain HPDMS;

[0055] Step 2: Synthesis of terminally allylated hindered phenols:

[0056] Under a nitrogen atmosphere at 0°C, 58 g of 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid and 16 g of 3-butene-1-ol were dissolved in 900 mL of dichloromethane and stirred for 10 min. 2 g of 4-dimethylaminopyridine was added and stirred for 10 min. 52 g of N,N-dicyclohexylcarbodiimide was dissolved in 200 mL of dichloromethane solution and added to the reaction system. After the reaction was completed, the reaction solution was poured into water, filtered and evaporated to obtain a crude product. The crude product was separated by silica gel column chromatography, eluted with an eluent consisting of 10 g of ethyl acetate and 90 g of cyclohexanone, and evaporated under reduced pressure at -0.2 MPa and 60°C for 2 h to obtain BBHP.

[0057] Step 3: Synthesis of hindered phenol modified silicone oil:

[0058] 50 g BBHP and 25 g HPDMS were added to a 250 mL dry three-necked flask equipped with a mixture meter, a stirrer and a condenser, and heated to 80 ° C. 6 g chloroplatinic acid was dissolved in 200 mL anhydrous ethanol and added to the three-necked flask. The solution temperature was raised to 120 ° C, bubbles were generated, and refluxed for 2 h to obtain hindered phenol-modified silicone oil.

[0059] Step 4: Synthesis of grease:

[0060] 40g of hindered phenol modified silicone oil, 15g of thickener, 0.75g of dithiodithiazolone, 0.75g of dialkyl copper dithiophosphate, 1.5g of T561 oxadiazole derivative and 4g of tetrabutylammonium chloride were put into a kneader, and low-temperature mixing and stirring were carried out at 90°C for 2h with a stirring speed of 50r / min; after the low-temperature mixing treatment was completed, the temperature was raised to 190°C, and stirring was carried out for 2h under a vacuum degree of 570mmHg with a stirring speed of 40r / min; the material was discharged and ground twice on a three-roll grinder to obtain grease.

[0061] Comparative Example 1

[0062] A method for preparing an antioxidant and high-temperature resistant grease, which is different from Example 2 in that the second and third steps are removed, and the "hindered phenol modified silicone oil" in the fourth step is replaced by "HPDMS", and the remaining raw materials and preparation process are the same as Example 2.

[0063] Comparative Example 2

[0064] A method for preparing an antioxidant and high-temperature resistant grease, which is different from Example 2 in that the third step is removed, and the "37g hindered phenol modified silicone oil" in the fourth step is replaced by "a mixture of 24.7g BBHP and 12.3g HPDMS", and the remaining raw materials and preparation process are the same as Example 2.

[0065] The performance of the grease obtained from Examples 1 to 3 and Comparative Examples 1 to 2 was tested, and the test items were as follows:

[0066] Table 1

[0067]

[0068] It can be seen from Table 1 that the grease prepared by the present invention has excellent oxidation resistance and high temperature resistance. The benzene ring structure in the hindered phenol and the active hydrogen on the hydroxyl group improve the thermal stability and oxidation resistance of the grease. The hindered phenol and the HPDMS silicone oil are combined together by chemical bonding, which effectively solves the problem of poor compatibility and easy precipitation of antioxidants in the matrix in the physical mixing method. In addition, the grease synthesized from the hindered phenol modified silicone oil as the base oil has a simple preparation process, is easy to control, has stable quality, and is suitable for industrial production.

[0069] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An antioxidant and high temperature resistant grease, characterized in that: The following raw materials are included by mass: Hindered phenol modified silicone oil 70-80 parts, thickener 10-30 parts, extreme pressure anti-wear agent 1-3 parts, anti-corrosion agent 1-3 parts, anti-fungal agent 2-8 parts; The hindered phenol modified silicone oil is prepared by the following method: BBHP and HPDMS are added into a three-necked flask, heated, and a Pt solution is added, and refluxed to obtain a hindered phenol-modified silicone oil, wherein BBHP is a terminal allylated hindered phenol, and HPDMS is a dihydrogen-terminated dimethyl polysiloxane.

2. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: HPDMS was prepared by the following method: Octamethylcyclotetrasiloxane, 1,1,3,3-tetramethyldisiloxane and acid clay were added into a three-necked flask, heated, and the acid clay was filtered off to obtain HPDMS.

3. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: BBHP was prepared by the following method: Under a nitrogen atmosphere, 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid and 3-butene-1-ol are dissolved in dichloromethane, stirred, and then 4-dimethylaminopyridine is added, stirred, and a dichloromethane solution containing N,N-dicyclohexylcarbodiimide is added. After the reaction is completed, the reaction solution is poured into water, filtered and evaporated to obtain a crude product. The crude product is separated by chromatography, eluted, and evaporated under reduced pressure to obtain BBHP.

4. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: The thickener is a powdered urea-based thickener, and the extreme pressure anti-wear agent is a complex of dithiodithiazolone and dialkyl copper dithiophosphate, and the mass ratio of dithiodithiazolone to dialkyl copper dithiophosphate is 1:

1.

5. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: The anticorrosive agent is at least one of T551 benzotriazole derivatives, T706 benzotriazole, and T561 oxadiazole derivatives, and the antifungal agent is at least one of 10,10'-oxybisphenoxane and tetrabutylammonium chloride.

6. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: The mass ratio of octamethylcyclotetrasiloxane, 1,1,3.3-tetramethyldisiloxane and acid clay is 15-20:1.7-2.4:0.5-1.

7. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: The usage ratio of 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid, 3-butene-1-ol, 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide is 5.2-5.8g: 1-1.6g: 0.18-0.20g: 4.6-5.2g.

8. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: The dosage ratio of N, N-dicyclohexylcarbodiimide to dichloromethane in the dichloromethane solution containing N, N-dicyclohexylcarbodiimide is 4.6-5.2 g: 10-20 mL.

9. The anti-oxidation and high temperature resistant grease according to claim 1, characterized in that: The dosage ratio of chloroplatinic acid and anhydrous ethanol in the Pt solution is 0.4-0.6 g:10-20 mL, and the mass ratio of BBHP, HPDMS and chloroplatinic acid is 50:25:4-6.

10. A method for preparing an antioxidant and high temperature resistant grease as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: Put hindered phenol modified silicone oil, thickener, extreme pressure anti-wear agent, corrosion inhibitor and mildew inhibitor into a kneader, mix and stir for 2 hours at 60-90°C, with a stirring speed of 40-50r / min; after the low-temperature mixing treatment is completed, heat up to 160-190°C, stir for 2 hours under a vacuum degree of 570mmHg, with a stirring speed of 30-40r / min; discharge the material, grind it twice with a three-roll grinder to obtain an antioxidant and high temperature resistant grease.