Method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel

By using vacuum nitrogen to cycle the molten steel during RH refining, the problem of difficult control of the nitrogen content in traditional steelmaking is solved, and natural nitrogen increase in the nitrogen content in molten steel is achieved, reducing production costs and improving the purity of molten steel.

CN119061240APending Publication Date: 2024-12-03PANGANG GRP XICHANG STEEL & VANADIUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411310729.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the traditional steelmaking process, the nitrogen content in the molten steel is difficult to control within the narrow range of 0.0025-0.0040%. The existing nitrogen-enhancing methods such as the use of manganese nitride alloys have stability problems, which affects production efficiency and molten steel purity, and workers work. High intensity.

Method used

During the RH refining process, vacuum nitrogen is used as the lifting gas for the steel water circulation, and argon is switched to nitrogen after the steel water is deoxygenated to achieve natural nitrogen increase in the steel water and control the nitrogen content between 0.0025-0.0040%.

Benefits of technology

Natural nitrogen increase in the nitrogen content in molten steel is achieved, which reduces production costs, improves the purity of molten steel, and reduces the labor intensity of workers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061240A_ABST
    Figure CN119061240A_ABST
Patent Text Reader

Abstract

The invention relates to a method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel. The method comprises the following steps that in the RH refining process, nitrogen is used in vacuum to serve as lifting gas for molten steel circulation; and the molten steel is alloyed for 3-10 min after being deoxidized, and the lifting gas is switched from argon to nitrogen. According to the nitrogen increasing method for the high-altitude vacuum non-alloyed molten steel, natural nitrogen increasing of the nitrogen content in the molten steel can be achieved in a non-alloyed mode, the production cost is reduced, meanwhile, the purity of the molten steel can be improved, and the labor intensity of workers can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steelmaking, in particular to the RH refining stage, and more particularly to a method for nitrogen addition to high-altitude vacuum non-alloyed molten steel. Background Art

[0002] In the steel manufacturing industry, in order to meet specific uses and performance requirements, it is often necessary to accurately control the content of various elements in steel. For example, in the production process of some special steel grades, the nitrogen content in the steel needs to be controlled within a very narrow range, such as 0.0025-0.0040%. This precise nitrogen content control is crucial to ensure the mechanical properties and welding performance of the steel.

[0003] In the traditional steelmaking process, the converter steelmaking method is usually used to produce basic molten steel, and then the molten steel composition is further adjusted through the refining process. However, the nitrogen content in the molten steel after the converter treatment is often lower than the required 0.0025%, which cannot meet the production requirements of the required steel grade. In the face of the situation where the nitrogen content is too low, in the traditional process method, manganese nitride alloy is often added to the molten steel to increase nitrogen. However, this method has three major disadvantages: First, the chemical properties of manganese nitride are unstable, it is easy to decompose, the nitrogen content is reduced, and it is not easy to preserve; second, due to the unstable nitrogen content of manganese nitride alloy, it is alloyed multiple times in the LF refining process, which affects the production efficiency and the purity of the molten steel; third, during alloying, a large amount of manual handling is required, and the labor intensity of workers is high.

[0004] In view of the above unfavorable factors, it is urgent to develop a method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel, which can reduce production costs, improve the purity of molten steel, and reduce the labor intensity of workers. Summary of the invention

[0005] In view of this, and in view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for increasing nitrogen in non-alloyed molten steel, which can reduce production costs, improve the purity of molten steel and reduce the labor intensity of workers, that is, to provide a method for increasing nitrogen in non-alloyed molten steel in a high-altitude vacuum.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions, which are specifically described as follows: According to aspects of the present invention, there is provided a method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel, comprising the following steps: Use nitrogen as a lifting gas for steel circulation in the RH refining process under vacuum; and After the molten steel is deoxidized and alloyed for 3-10 minutes, the lifting gas is switched from argon to nitrogen.

[0007] In one embodiment of the present invention, when nitrogen is used as the lifting gas, the lifting gas flow rate is set to 2200-2600 NL / min during nitrogen blowing.

[0008] In one embodiment of the present invention, the vacuum molten steel circulation is terminated after nitrogen blowing for 3 minutes.

[0009] In one embodiment of the present invention, the high altitude is above 4000 m above sea level.

[0010] In one embodiment of the present invention, a RH vacuuming step is further included before using nitrogen as a lifting gas for molten steel circulation in vacuum.

[0011] In one embodiment of the present invention, the RH vacuuming time is 8-10 minutes.

[0012] In one embodiment of the present invention, the lifting gas is switched from argon to nitrogen after the molten steel is alloyed for 5 minutes after deoxidation.

[0013] In one embodiment of the present invention, the nitrogen gas is anhydrous nitrogen gas with a purity of 99.9%.

[0014] In one embodiment of the present invention, nitrogen is circulated in the molten steel to achieve natural nitrogen enrichment during the molten steel treatment process.

[0015] In one embodiment of the present invention, the nitrogen content in the molten steel is controlled at 0.0025-0.0040%.

[0016] By adopting the above technical solution, the present invention has the following advantages compared with the prior art: The present invention provides a method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel, which can achieve natural increase of nitrogen content in molten steel by non-alloying. This method can reduce production costs, improve the purity of molten steel, and reduce the labor intensity of workers. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.

[0018] The above and / or additional aspects and advantages of the present invention will be more obvious and easily understood in the description of the embodiments in conjunction with the accompanying drawings, in which: Figure 1 A schematic flow chart of a method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention is shown. DETAILED DESCRIPTION

[0019] It should be understood that the embodiments of the present invention shown in the exemplary embodiments are only illustrative. Although only a few embodiments are described in detail in the present invention, it is easy for those skilled in the art to appreciate that multiple modifications are feasible without actually departing from the teaching of the subject matter of the present invention. Accordingly, all such modifications should be included within the scope of the present invention. Without departing from the gist of the present invention, other replacements, modifications, changes and deletions may be made to the design, operating conditions and parameters of the following exemplary embodiments.

[0020] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0021] Figure 1 The schematic diagram of the process of nitrogen addition in high altitude vacuum non-alloyed molten steel provided by the present invention is shown. Figure 1 As shown, the present invention provides a method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel, comprising the following steps: S101: Nitrogen is used as lifting gas for steel circulation in vacuum during RH refining; S102: After the molten steel is deoxidized and alloyed for 3-10 minutes, the lifting gas is switched from argon to nitrogen.

[0022] Based on the above technical scheme, the method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention can achieve natural nitrogen increase of the nitrogen content in the molten steel by non-alloying means. This method can reduce production costs while improving the purity of the molten steel and reducing the labor intensity of workers.

[0023] In a preferred embodiment of a method for increasing nitrogen in a high-altitude vacuum non-alloyed molten steel provided by the present invention, when nitrogen is used as a lifting gas, the range of the lifting gas flow rate during nitrogen blowing is set to 2200-2600NL / min. More preferably, the lifting gas flow rate during nitrogen blowing can be set to 2200NL / min, 2500NL / min or 2600NL / min.

[0024] In a preferred embodiment of the method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention, the vacuum molten steel circulation is terminated after blowing nitrogen for 3 minutes. For example, the vacuum molten steel circulation can be terminated after blowing nitrogen for 4 minutes, 5 minutes or 6 minutes. In a preferred embodiment of the method for increasing nitrogen in vacuum non-alloyed molten steel at high altitude provided by the present invention, the high altitude is above 4000 m above sea level. For example, the high altitude is preferably 5000 m or 8000 m above sea level.

[0025] In a preferred embodiment of the method for increasing nitrogen in non-alloyed molten steel in vacuum at high altitude provided by the present invention, a RH vacuuming step is also included before nitrogen is used as a lifting gas for the circulation of molten steel in vacuum.

[0026] In the preferred embodiment of the method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention, the RH vacuum pumping time is 8-10 minutes, preferably 10 minutes.

[0027] In a preferred embodiment of the method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention, the lifting gas can be switched from argon to nitrogen after the molten steel is alloyed for 5 minutes after deoxidation. Of course, it is also preferred to switch the lifting gas from argon to nitrogen after the molten steel is alloyed for 8 minutes after deoxidation.

[0028] In a preferred embodiment of the method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention, the nitrogen gas used is anhydrous nitrogen gas with a purity of 99.9%.

[0029] In the preferred embodiment of the method for increasing nitrogen in high altitude vacuum non-alloyed molten steel provided by the present invention, nitrogen is circulated in the molten steel to achieve natural nitrogen increase during the molten steel treatment process. In this embodiment, no alloy is needed to increase the nitrogen content, but nitrogen is used to achieve natural nitrogen increase.

[0030] In a preferred embodiment of the method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention, the nitrogen content in the molten steel is controlled at 0.0025-0.0040%. More preferably, the nitrogen content in the molten steel is 0.0025%.

[0031] The scheme of the present invention will be explained below in conjunction with embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. Where specific techniques or conditions are not specified in the embodiments, conventional techniques in the art are followed.

[0032] In an embodiment of the present invention, a method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel is provided, and the specific scheme is as follows: Carry out RH vacuum for 8-10min. At an altitude of more than 4000m, use 99.9% anhydrous nitrogen as the lifting gas for molten steel circulation in vacuum during RH refining, and switch the lifting gas from argon to nitrogen for 3-10min after the molten steel is deoxidized and alloyed. Set the lifting gas flow rate to 2200-2600NL / min during nitrogen blowing, and terminate the vacuum molten steel circulation after 3min of nitrogen blowing. After nitrogen circulates in the molten steel, natural nitrogen increase in the molten steel treatment process is achieved, and the nitrogen content in the molten steel is controlled at 0.0025-0.0040%.

[0033] Example 1 This embodiment produces a steel grade with a nitrogen content controlled to 0.0030%. RH vacuuming is performed for 8 minutes, at an altitude of 4000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after alloying for 3 minutes after deoxidation of the molten steel. The lifting gas flow rate is set to 2200NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 4 minutes. After nitrogen circulates in the molten steel, natural nitrogen increase is achieved during the molten steel treatment process, and the nitrogen content in the molten steel is controlled at 0.0030%.

[0034] Example 2 This embodiment produces a steel grade with a nitrogen content controlled to 0.0025%. RH vacuuming is performed for 9 minutes, at an altitude of 5000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after alloying for 6 minutes after deoxidation of the molten steel. The lifting gas flow rate is set to 2400NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 5 minutes. After nitrogen circulates in the molten steel, natural nitrogen increase is achieved during the molten steel treatment process, and the nitrogen content in the molten steel is controlled at 0.0025%.

[0035] Example 3 This embodiment needs to produce a steel grade with a nitrogen content controlled to 0.0040%. RH vacuuming is performed for 10 minutes, at an altitude of 8000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after the molten steel is deoxidized and alloyed for 4 minutes. The lifting gas flow rate is set to 2600NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 4 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled at 0.0040%.

[0036] Example 4 This embodiment needs to produce a steel grade with a nitrogen content controlled to 0.0028%. RH vacuuming is performed for 10 minutes, at an altitude of 5000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen for 10 minutes after the molten steel is deoxidized and alloyed. The lifting gas flow rate is set to 2300NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 3 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled at 0.0025%.

[0037] Example 5 This embodiment produces a steel grade with a nitrogen content controlled to 0.0035%. RH vacuuming is performed for 9 minutes, at an altitude of 6000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after alloying for 8 minutes after deoxidation of the molten steel. The lifting gas flow rate is set to 2400NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 5 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled at 0.0035%.

[0038] Example 6 This embodiment produces a steel grade with a nitrogen content controlled to 0.0025%. RH vacuuming is performed for 10 minutes, at an altitude of 5000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after the molten steel is deoxidized and alloyed for 4 minutes. The lifting gas flow rate is set to 2450NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 5 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled to 0.0025%.

[0039] Example 7 This embodiment produces a steel grade with a nitrogen content controlled to 0.0025%. RH vacuuming is performed for 9 minutes, at an altitude of 8000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after the molten steel is deoxidized and alloyed for 8 minutes. The lifting gas flow rate is set to 2320NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 4 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled to 0.0025%.

[0040] Example 8 This embodiment produces a steel grade with a nitrogen content controlled to 0.0028%. RH vacuuming is performed for 8 minutes, at an altitude of 6000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after the molten steel is deoxidized and alloyed for 4 minutes. The lifting gas flow rate is set to 2550NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 6 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled to 0.0028%.

[0041] Example 9 This embodiment produces a steel grade with a nitrogen content controlled to 0.0032%. RH vacuuming is performed for 8 minutes, at an altitude of 7000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after the molten steel is deoxidized and alloyed for 6 minutes. The lifting gas flow rate is set to 2580NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 3 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled to 0.0032%.

[0042] Example 10 This embodiment produces a steel grade with a nitrogen content controlled to 0.0036%. RH vacuuming is performed for 10 minutes, at an altitude of 4000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after the molten steel is deoxidized and alloyed for 4 minutes. The lifting gas flow rate is set to 2590NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 5 minutes. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled to 0.0036%.

[0043] Embodiment 11 This embodiment produces a steel grade with a nitrogen content controlled to 0.0038%. RH vacuuming is performed for 9 minutes, at an altitude of 6000m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen after alloying for 7 minutes after deoxidation of the molten steel. The lifting gas flow rate is set to 2600NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after nitrogen blowing for 5 minutes. After nitrogen circulates in the molten steel, natural nitrogen increase is achieved during the molten steel treatment process, and the nitrogen content in the molten steel is controlled at 0.0038%.

[0044] Example 12 This embodiment produces a steel grade with a nitrogen content controlled to 0.0040%. RH vacuuming is performed for 8.5 minutes, at an altitude of 6500m, 99.9% anhydrous nitrogen is used as the lifting gas for molten steel circulation in the vacuum during RH refining, and the lifting gas is switched from argon to nitrogen for 4.5 minutes after the molten steel is deoxidized and alloyed. The lifting gas flow rate is set to 2580NL / min during nitrogen blowing, and the vacuum molten steel circulation is terminated after 4.5 minutes of nitrogen blowing. After nitrogen circulates in the molten steel, natural nitrogen is added during the molten steel treatment process, and the nitrogen content in the molten steel is controlled to 0.0040%.

[0045] It can be seen that in the method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel provided by the present invention, a non-alloying method is used to achieve natural nitrogen increase in the nitrogen content in the molten steel, and the nitrogen content of the steel grade can be controlled at 0.0025-0.0040%, not less than 0.0025%, thereby meeting the production requirements of the steel grade.

[0046] In addition, in the above method of the present invention, for example, manganese nitride alloy is not used for nitrogen addition. Instead, the lifting gas is directly switched from argon to nitrogen after the molten steel is deoxidized and alloyed for 3-10 minutes, and vacuum is used as the lifting gas for the molten steel circulation, thereby overcoming the defects of using alloy to increase nitrogen. That is, the method of the present invention can improve the purity of molten steel and reduce the labor intensity of workers while reducing production costs.

[0047] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusions, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to the process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "including a..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0048] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0049] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel, characterized in that: The following steps are involved: Use nitrogen as a lifting gas for steel circulation in the RH refining process under vacuum; and After the molten steel is deoxidized and alloyed for 3-10 minutes, the lifting gas is switched from argon to nitrogen.

2. The method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel according to claim 1, characterized in that: When nitrogen is used as the lifting gas, the lifting gas flow rate is set to 2200-2600NL / min during nitrogen blowing.

3. The method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel according to claim 2, characterized in that: After blowing nitrogen for 3 minutes, the vacuum molten steel circulation was terminated.

4. The method for increasing nitrogen in high-altitude vacuum non-alloyed molten steel according to claim 1, characterized in that: The high altitude is above 4000m above sea level.

5. The method for increasing nitrogen in high altitude vacuum non-alloyed molten steel according to claim 1, characterized in that: A RH evacuation step is also included before vacuum using nitrogen as a lift gas for the molten steel circulation.

6. The method for increasing nitrogen in high altitude vacuum non-alloyed molten steel according to claim 5, characterized in that: RH vacuuming time is 8-10min.

7. The method for increasing nitrogen in high altitude vacuum non-alloyed molten steel according to claim 1, characterized in that: After the molten steel is deoxidized and alloyed for 5 minutes, the lifting gas is switched from argon to nitrogen.

8. The method for increasing nitrogen in high altitude vacuum non-alloyed molten steel according to claim 1, characterized in that: The nitrogen gas is anhydrous nitrogen gas with a purity of 99.9%.

9. The method for increasing nitrogen in high altitude vacuum non-alloyed molten steel according to claim 1, characterized in that: After nitrogen circulates in the molten steel, natural nitrogen addition is achieved during the molten steel treatment process.

10. The method for increasing nitrogen in high altitude vacuum non-alloyed molten steel according to claim 9, characterized in that: The nitrogen content in molten steel is controlled at 0.0025-0.0040%.