Method for improving forming performance of hot-galvanized ultrahigh-strength dual-phase steel
The method of continuous annealing and aging transforms primary martensite into tempered martensite in galvanized dual-phase steel, addressing formability issues by reducing hardness differences and improving phase interface compatibility, thereby enhancing hole expansion and bending performance.
Patent Information
- Application Number
- CN202411118370.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-12-03
AI Technical Summary
The formability, particularly local formability, of ultra-high-strength galvanized dual-phase steel has deteriorated due to the reduction of expensive alloying elements like Mo, making it difficult to meet the forming requirements of automotive parts, especially in terms of hole expansion and bending performance.
A method involving continuous annealing of cold-hardened steel strips, including heating, slow cooling, rapid cooling, and aging to transform primary martensite into tempered martensite, followed by hot-dip galvanizing, to reduce hardness differences and improve phase interface compatibility.
Significantly enhances the hole expansion and bending performance of hot-dip galvanized ultra-high strength dual-phase steel by reducing hardness disparities and inharmonious deformation, achieving improvements of over 50% in hole expansion and 57-106% in bending performance compared to conventional processes.
Smart Images

Figure CN119061252A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of automobile steel and engineering structure steel, and in particular to a method for improving the forming performance of hot-dip galvanized ultra-high strength dual-phase steel. Background Art
[0002] Due to the advantages of low yield-to-strength ratio, good comprehensive formability and low cost, dual-phase steel (DP steel) has become the most widely used steel type in white body.
[0003] However, as the requirements for automobile energy conservation, emission reduction and safety become more and more stringent, the automotive industry has an increasingly urgent demand for high-strength steel with higher elongation and formability. In addition, competition in the automotive industry is becoming increasingly fierce, and the pressure to reduce costs is gradually being passed on to upstream industries. Against this background, the development of ultra-high-strength DP steel with low cost and high formability has become an urgent task for the steel industry. About 0.2% Mo is usually added to DP steel. On the one hand, the Mo element can improve the hardenability of the material, and on the other hand, it can also improve the bonding force of the grain boundaries, which is beneficial to the formability of the material. However, with the reduction of expensive alloying elements such as Mo in galvanized high-strength steel, its formability, especially the local formability, has deteriorated significantly, making it difficult to meet the forming requirements of some parts. Therefore, there is an urgent need for a method to improve the formability of ultra-high-strength galvanized DP steel. Summary of the invention
[0004] The present application provides a method for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel to solve the following technical problem: how to improve the formability of hot-dip galvanized ultra-high strength dual-phase steel.
[0005] In a first aspect, the present application provides a method for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel, the method comprising:
[0006] The cold-hardened strip steel is continuously annealed to obtain an annealed sheet;
[0007] The method of continuously annealing the cold hardened steel strip to obtain the annealed sheet comprises:
[0008] heating the chilled steel strip to a first temperature for soaking;
[0009] Slowly cooling the steel strip after the soaking, and then rapidly cooling it to a second temperature, so that a sufficient amount of primary martensite is generated in the structure of the steel strip after the slow cooling;
[0010] Heating the rapidly cooled steel strip to a third temperature for aging, so that the primary martensite in the structure of the rapidly cooled steel strip is transformed into tempered martensite to obtain an annealed sheet;
[0011] The annealed sheet is hot-dip galvanized to obtain hot-dip galvanized ultra-high strength dual-phase steel.
[0012] Optionally, the first temperature is 780°C to 830°C.
[0013] Optionally, the second temperature is 220°C to 380°C.
[0014] Optionally, the third temperature is 250°C to 400°C.
[0015] Optionally, the temperature of the hot-dip galvanizing pot is 440°C to 460°C.
[0016] Optionally, the running speed of the strip steel in the continuous annealing is 70 mpm to 120 mpm.
[0017] Optionally, the microstructure of the hot-dip galvanized ultra-high strength steel includes tempered martensite, ferrite, fresh martensite and bainite.
[0018] Optionally, the hot-dip galvanized ultra-high strength steel is a 780MPa grade hot-dip galvanized duplex steel;
[0019] The volume fraction of the ferrite is 60% to 70%, and the average grain size of the ferrite is not greater than 5 μm;
[0020] The volume fraction of the tempered martensite is 20% to 25%, and the grain size of the tempered martensite is not greater than 2 μm;
[0021] The volume fraction of the fresh martensite is 5% to 10%, and the grain size of the fresh martensite is not greater than 2 μm;
[0022] The volume fraction of the bainite is 4% to 5%, and the grain size of the bainite is no greater than 1.5 μm.
[0023] Optionally, the hot-dip galvanized ultra-high strength steel is a 980MPa grade hot-dip galvanized duplex steel;
[0024] The volume fraction of the ferrite is 50-60%, and the average grain size of the ferrite is not greater than 4.5 μm;
[0025] The volume fraction of the tempered martensite is 25% to 30%, and the grain size of the tempered martensite is not greater than 2 μm;
[0026] The volume fraction of the fresh martensite is 5% to 15%, and the grain size of the fresh martensite is not greater than 2 μm;
[0027] The volume fraction of the bainite is 4% to 5%, and the grain size of the bainite is no greater than 1.5 μm.
[0028] Optionally, the hot-dip galvanized ultra-high strength steel is a 1180MPa grade hot-dip galvanized duplex steel;
[0029] The volume fraction of the ferrite is 30% to 50%, and the average grain size of the ferrite is not greater than 4 μm;
[0030] The volume fraction of the tempered martensite is 40-45%, and the grain size of the tempered martensite is not greater than 2 μm;
[0031] The volume fraction of the fresh martensite is 5% to 15%, and the grain size of the fresh martensite is not greater than 2 μm;
[0032] The volume fraction of the bainite is 5% to 7%, and the grain size of the bainite is no greater than 1.0 μm.
[0033] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0034] The method for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel provided in an embodiment of the present application comprises: continuously annealing a cold-hardened steel strip to obtain an annealed plate; the continuous annealing of the cold-hardened steel strip to obtain an annealed plate comprises: heating the cold-hardened steel strip to a first temperature for uniform heating; slowly cooling the steel strip after uniform heating, and then rapidly cooling to a second temperature, so that a sufficient amount of primary martensite is generated in the structure of the steel strip after the slow cooling; heating the steel strip after the rapid cooling to a third temperature for aging, so that the primary martensite in the structure of the steel strip after the rapid cooling is transformed into tempered martensite to obtain an annealed plate; hot-dip galvanizing the annealed plate to obtain a hot-dip galvanized ultra-high strength dual-phase steel. The cold-hardened steel strip is heated to a first temperature for uniform heating, so that the cold-hardened steel strip has ideal strength properties; after slow cooling and rapid cooling, it is cooled to a second temperature, that is, a temperature below the Ms point and significantly lower than the zinc pot temperature, so that a sufficient amount of primary martensite can be generated in the structure of the slow-cooled steel strip; the rapidly cooled steel strip is heated to a third temperature for aging, and the primary martensite is tempered, thereby reducing the hardness of the martensite and improving the degree of inharmonious deformation of the ferrite / martensite phase interface, so that the steel strip has high forming performance; the annealed sheet is hot-dip galvanized to obtain hot-dip galvanized ultra-high strength dual-phase steel with ideal structure. This method reduces the hardness difference of the ferrite / fresh martensite phase and the inharmonious deformation of the interface of the two phases, effectively resists the initiation and expansion of cracks in the hot-dip galvanized ultra-high strength dual-phase steel during the deformation process, thereby significantly improving the hole expansion and bending performance of the hot-dip galvanized ultra-high strength dual-phase steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0037] Figure 1 A schematic flow chart of a method for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel according to some embodiments of the present application;
[0038] Figure 2 A schematic diagram of a continuous annealing process of hot-dip galvanized ultra-high strength dual-phase steel provided in accordance with a comparative example of the present application;
[0039] Figure 3 A schematic diagram of a continuous annealing process of hot-dip galvanized ultra-high strength dual-phase steel according to an embodiment of the present application;
[0040] Figure 4 The microstructure of the 980MPa grade hot-dip galvanized ultra-high strength dual-phase steel provided in the comparative example of the present application;
[0041] Figure 5 The microstructure of 980MPa grade hot-dip galvanized ultra-high strength dual-phase steel provided according to the embodiment of the present application. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0043] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0044] In this application, the terms "including", "comprising", etc. mean "including but not limited to".
[0045] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0046] Under conventional galvanizing process conditions, the rapid cooling temperature of the steel strip is basically equal to the temperature of entering the zinc pot, and the final structure of the steel strip is composed of ferrite, fresh martensite and a small amount of bainite. Since the fresh martensite has not been tempered, it has a high hardness, and the hardness difference between it and ferrite is very large. During the deformation process, due to the inharmonious deformation of the ferrite / fresh martensite phase interface, cracks can easily initiate and expand at the phase interface. For Mo-containing DP steel, its formability is acceptable because the Mo element has the effect of improving the bonding strength of the phase interface and refining the grains; but for low-cost high-strength steel without Mo, its hole expansion rate and bending performance will drop to a level that customers cannot accept. In order to improve the formability of such high-strength steel, the primary issue is to reduce the hardness difference and strain incompatibility level between the soft phase / hard phase, and this goal can be achieved by improving the existing annealing process. Therefore, the present application provides a method for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel, Figure 1 A schematic diagram of a method for improving the forming performance of hot-dip galvanized ultra-high strength dual-phase steel according to some embodiments of the present application; see Figure 1 , the method comprising:
[0047] S1, continuously annealing the cold hardened strip steel to obtain an annealed plate;
[0048] The method of continuously annealing the cold hardened steel strip to obtain the annealed sheet comprises:
[0049] heating the chilled steel strip to a first temperature for soaking;
[0050] Slowly cooling the steel strip after the soaking, and then rapidly cooling it to a second temperature, so that a sufficient amount of primary martensite is generated in the structure of the steel strip after the slow cooling;
[0051] Heating the rapidly cooled steel strip to a third temperature for aging, so that the primary martensite in the structure of the rapidly cooled steel strip is transformed into tempered martensite to obtain an annealed sheet;
[0052] In some embodiments, the first temperature is 780°C to 830°C.
[0053] In some embodiments, the second temperature is 220°C to 380°C.
[0054] In some embodiments, the third temperature is 250°C to 400°C.
[0055] In some embodiments, the running speed of the steel strip during the continuous annealing is 70 mpm to 120 mpm.
[0056] In the embodiment of the present application, after the steel strip is heated, soaked and slowly cooled, it is rapidly cooled to a temperature below the Ms point and significantly lower than the zinc pot temperature to obtain the required volume fraction of primary martensite; then the steel strip is heated to a certain temperature for aging to temper the primary martensite. After the new annealing process, the hardness difference between the soft phase / hard phase of the steel strip can be significantly reduced, which can effectively resist the initiation and expansion of cracks during deformation, thereby significantly improving the hole expansion and bending performance of the material. Limiting the soaking temperature of continuous annealing can ensure the high strength of the steel strip; limiting the rapid cooling temperature can generate a sufficient amount of primary martensite in the organization of the steel strip; the aging process tempers the primary martensite formed in the rapid cooling stage, thereby reducing the hardness of the martensite, improving the degree of deformation incompatibility of the ferrite / martensite phase interface, and facilitating the acquisition of high forming performance. "First temperature" represents soaking temperature, "second temperature" represents rapid cooling temperature, and "third temperature" represents aging temperature. For example, the soaking temperature may be 780°C, 785°C, 790°C, 795°C, 800°C, 805°C, 810°C, 815°C, 820°C, 825°C, 830°C, etc., and the rapid cooling temperature may be 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, etc. The aging temperature may be 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, etc. The aging time can be 0.5min to 1min, and a good tempering effect can be obtained. Furthermore, the running speed of the strip in the above continuous annealing can be 70mpm, 80mpm, 90mpm, 100, 110mpm, 120mpm, etc. The above slow cooling temperature can be 680℃ to 740℃. For example, Figure 2 A schematic diagram of a continuous annealing process of hot-dip galvanized ultra-high strength dual-phase steel provided in accordance with a comparative example of the present application; Figure 3 Schematic diagram of the continuous annealing process of hot-dip galvanized ultra-high strength dual-phase steel provided in accordance with the embodiment of the present application; see Figures 2-3 .
[0057] In addition, before the above step S1, the continuous casting billet is cleaned and then hot-charged into a furnace, and the continuous casting billet is heated, rolled, coiled, pickled and cold-rolled to obtain a cold-hardened strip steel. The heating temperature can be 1150-1250°C, which can make the steel structure homogenized and the micro-alloy elements fully dissolved, avoiding abnormal grain growth; the hot rolling final rolling temperature can be 900°C, which can make the steel structure homogenized and the micro-alloy elements fully dissolved, avoiding abnormal grain growth; the coiling temperature can be 250°C, which can obtain a full martensitic structure in the steel.
[0058] S2. Hot-dip galvanizing the annealed sheet to obtain hot-dip galvanized ultra-high strength dual-phase steel.
[0059] In some embodiments, the temperature of the hot-dip galvanizing pot is 440°C to 460°C.
[0060] In the embodiment of the present application, limiting the zinc pot temperature for hot-dip galvanizing can ensure good quality of the zinc coating. For example, the zinc pot temperature can be 440°C, 445°C, 450°C, 455°C, 460°C, etc.
[0061] In some embodiments, the microstructure of the hot-dip galvanized ultra-high strength steel includes tempered martensite, ferrite, fresh martensite and bainite.
[0062] In some embodiments, the hot-dip galvanized ultra-high strength steel is a 780MPa grade hot-dip galvanized dual-phase steel;
[0063] The volume fraction of the ferrite is 60% to 70%, and the average grain size of the ferrite is not greater than 5 μm;
[0064] The volume fraction of the tempered martensite is 20% to 25%, and the grain size of the tempered martensite is not greater than 2 μm;
[0065] The volume fraction of the fresh martensite is 5% to 10%, and the grain size of the fresh martensite is not greater than 2 μm;
[0066] The volume fraction of the bainite is 4% to 5%, and the grain size of the bainite is no greater than 1.5 μm.
[0067] In some embodiments, the hot-dip galvanized ultra-high strength steel is a 980 MPa grade hot-dip galvanized dual-phase steel;
[0068] The volume fraction of the ferrite is 50-60%, and the average grain size of the ferrite is not greater than 4.5 μm;
[0069] The volume fraction of the tempered martensite is 25% to 30%, and the grain size of the tempered martensite is not greater than 2 μm;
[0070] The volume fraction of the fresh martensite is 5% to 15%, and the grain size of the fresh martensite is not greater than 2 μm;
[0071] The volume fraction of the bainite is 4% to 5%, and the grain size of the bainite is no greater than 1.5 μm.
[0072] In some embodiments, the hot-dip galvanized ultra-high strength steel is a 1180 MPa grade hot-dip galvanized dual-phase steel;
[0073] The volume fraction of the ferrite is 30% to 50%, and the average grain size of the ferrite is not greater than 4 μm;
[0074] The volume fraction of the tempered martensite is 40-45%, and the grain size of the tempered martensite is not greater than 2 μm;
[0075] The volume fraction of the fresh martensite is 5% to 15%, and the grain size of the fresh martensite is not greater than 2 μm;
[0076] The volume fraction of the bainite is 5% to 7%, and the grain size of the bainite is no greater than 1.0 μm.
[0077] In the embodiment of the present application, the hot-dip galvanized ultra-high strength steel can be 780MPa-1180MPa grade DP steel, and the microstructure of the strip steel includes tempered martensite, ferrite, fresh martensite and a small amount of bainite, and has the characteristics of fine grain size. Using the above method for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel, the hole expansion rate and V-bend performance of the hot-dip galvanized DP steel of 780MPa grade and above of the existing composition system are improved by more than 50%.
[0078] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0079] The embodiment of the present application provides a method for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel. Please refer to the process parameters for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel shown in Table 1.
[0080] Table 1 Process parameters for improving the formability of hot-dip galvanized ultra-high strength dual-phase steel
[0081]
[0082]
[0083] The hot-dip galvanized ultra-high strength dual-phase steels obtained in Examples 1 to 18 and Comparative Examples 1 to 3 were subjected to performance and microstructure tests. Please refer to Table 2 for the microstructure of the hot-dip galvanized ultra-high strength dual-phase steels, and Table 3 for the performance of the hot-dip galvanized ultra-high strength dual-phase steels.
[0084] Table 2 Microstructure of hot-dip galvanized ultra-high strength dual-phase steel
[0085]
[0086]
[0087] Table 3 Properties of hot-dip galvanized ultra-high strength dual-phase steel
[0088]
[0089]
[0090] According to Tables 2 and 3, Comparative Examples 1 to 6 and Example 1 correspond to DP780. Comparative Example 1 is a conventional hot-dip galvanized ultra-high strength dual-phase steel preparation process. It can be seen that although the mechanical properties meet the standard requirements under the conventional process, the hole expansion rate is only 16%, the V-bend radius is also large, and the bending performance is low. The soaking temperature of Comparative Example 2 is too low, resulting in a tensile strength lower than 780MPa, but after the rapid cooling temperature drops, the hole expansion and bending performance are significantly improved. The soaking temperature of Comparative Example 3 is too high, resulting in high tensile strength and low elongation. The rapid cooling temperature of process 4 is too low, resulting in excessive primary martensite content and low tensile strength after tempering. The rapid cooling temperature of Comparative Example 5 is too high, resulting in less tempered martensite content and limited improvement in hole expansion. The aging temperature of Comparative Example 6 is too high, resulting in low tensile strength. The process parameters of Example 1 are within the scope of the embodiments of the present application, the mechanical properties meet the requirements, and the forming performance is good. The hole expansion and bending performance are improved by 94% and 75% respectively compared with the conventional galvanizing process.
[0091] Comparative Examples 7 to 12 and Example 2 correspond to DP980. Comparative Example 7 is a conventional galvanizing process. Like DP780, it also has the problem that the mechanical properties are qualified but the hole expansion and bending properties are low. Comparative Example 8 has too low agitation, resulting in inadequate tensile strength. Comparative Example 9 has too high agitation, resulting in high tensile strength. Comparative Example 10 has too low rapid cooling temperature, resulting in low tensile strength. Comparative Example 11 has too high a rapid cooling temperature, resulting in limited improvement in hole expansion and bending properties. Comparative Example 12 has too high an aging temperature, resulting in low tensile strength. The process parameters of Example 2 are within the scope of the embodiments of this application, the mechanical properties meet the standard requirements, and the hole expansion and bending properties are improved by 106% and 60% respectively compared with conventional galvanizing processes. For example, Figure 4 For the microstructure of 980MPa grade hot-dip galvanized ultra-high strength dual-phase steel provided in the comparative example of this application, please refer to Figure 4 , including ferrite, fresh martensite and a small amount of bainite; Figure 5 For the microstructure of the 980MPa grade hot-dip galvanized ultra-high strength dual-phase steel provided in the embodiment of the present application, please refer to Figure 5 , including ferrite, fresh martensite, tempered martensite and a small amount of bainite.
[0092] Comparative Examples 13 to 18 and Example 3 correspond to DP1180. Compared with the conventional galvanizing process, the process parameters of Example 3 are within the scope of the embodiments of the present application, and the hole expansion and bending performance are improved by 58% and 57% respectively.
[0093] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for improving the forming performance of hot-dip galvanized ultra-high strength dual-phase steel, characterized in that: The method comprises: The cold-hardened strip steel is continuously annealed to obtain an annealed sheet; The method of continuously annealing the cold hardened steel strip to obtain the annealed sheet comprises: heating the chilled steel strip to a first temperature for soaking; Slowly cooling the steel strip after the soaking, and then rapidly cooling it to a second temperature, so that a sufficient amount of primary martensite is generated in the structure of the steel strip after the slow cooling; Heating the rapidly cooled steel strip to a third temperature for aging, so that the primary martensite in the structure of the rapidly cooled steel strip is transformed into tempered martensite to obtain an annealed sheet; The annealed sheet is hot-dip galvanized to obtain hot-dip galvanized ultra-high strength dual-phase steel.
2. The method according to claim 1, characterized in that The first temperature is 780°C to 830°C.
3. The method according to claim 1, characterized in that The second temperature is 220°C to 380°C.
4. The method according to claim 1, characterized in that: The third temperature is 250°C to 400°C.
5. The method according to claim 1, characterized in that The temperature of the hot-dip galvanizing pot is 440°C to 460°C.
6. The method according to claim 1, characterized in that The running speed of the strip during the continuous annealing is 70 mpm to 120 mpm.
7. The method according to claim 1, characterized in that The microstructure of the hot-dip galvanized ultra-high strength steel includes tempered martensite, ferrite, fresh martensite and bainite.
8. The method according to claim 7, characterized in that The hot-dip galvanized ultra-high strength steel is a 780MPa grade hot-dip galvanized dual-phase steel; The volume fraction of the ferrite is 60% to 70%, and the average grain size of the ferrite is not greater than 5 μm; The volume fraction of the tempered martensite is 20% to 25%, and the grain size of the tempered martensite is not greater than 2 μm; The volume fraction of the fresh martensite is 5% to 10%, and the grain size of the fresh martensite is not greater than 2 μm; The volume fraction of the bainite is 4% to 5%, and the grain size of the bainite is no greater than 1.5 μm.
9. The method according to claim 7, characterized in that: The hot-dip galvanized ultra-high strength steel is a 980MPa grade hot-dip galvanized dual-phase steel; The volume fraction of the ferrite is 50-60%, and the average grain size of the ferrite is not greater than 4.5 μm; The volume fraction of the tempered martensite is 25% to 30%, and the grain size of the tempered martensite is not greater than 2 μm; The volume fraction of the fresh martensite is 5% to 15%, and the grain size of the fresh martensite is not greater than 2 μm; The volume fraction of the bainite is 4% to 5%, and the grain size of the bainite is no greater than 1.5 μm.
10. The method according to claim 7, characterized in that The hot-dip galvanized ultra-high strength steel is a 1180MPa grade hot-dip galvanized dual-phase steel; The volume fraction of the ferrite is 30% to 50%, and the average grain size of the ferrite is not greater than 4 μm; The volume fraction of the tempered martensite is 40-45%, and the grain size of the tempered martensite is not greater than 2 μm; The volume fraction of the fresh martensite is 5% to 15%, and the grain size of the fresh martensite is not greater than 2 μm; The volume fraction of the bainite is 5% to 7%, and the grain size of the bainite is no greater than 1.0 μm.
Citation Information
Patent Citations
Cold-rolled hot-galvanized duplex steel and manufacturing method thereof
CN110093491A
Hot-dip galvanized DH steel, preparation method thereof and automobile structural member
CN116397158A
Continuous annealing method of dual-phase steel with enhanced formability and preparation method of dual-phase steel
CN117512281A
Annealing process for improving broaching performance of 800 MPa-grade dual-phase steel
CN117512282A
1180MPa-grade hot-dip galvanized dual-phase steel and preparation method thereof
CN118064801A