Continuous annealing device and method

By adding the second fast cooling section and the second aging section to the traditional continuous annealing production line, multiple cooling and aging treatments of strip steel are controlled, and the problem of insufficient forming performance of the third-generation high-strength steel is solved, which significantly improves the elongation and The pore reaming rate meets the forming needs of complex parts and takes into account the production of existing steel grades.

CN119061254APending Publication Date: 2024-12-03SHOUGANG GROUP CO LTD

Patent Information

Application Number
CN202411229218.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional third-generation high-strength steels are difficult to meet the needs of complex parts in forming performance, especially in areas with large strains, which are prone to cracking. As the strength level increases, their elongation gradually decreases, making it difficult to meet the requirements of high forming performance.

Method used

On the basis of the traditional continuous annealing production line, the second fast cooling section and the second aging section are added, through the heating section, the heat homogenization section, the slow cooling section, the first fast cooling section, the first aging section, the second fast cooling section and The combined treatment of the second aging section controls multiple cooling and aging treatments of the strip, improves its elongation and pore reaming rate, and thereby improves the forming performance.

Benefits of technology

It significantly improves the elongation and pore reaming rate of the third generation of high-strength steel, improves the forming performance, so that it can meet the forming needs of complex parts, while taking into account the production process of existing steel grades, achieving higher forming performance and compatibility. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061254A_ABST
    Figure CN119061254A_ABST
Patent Text Reader

Abstract

The invention discloses a continuous annealing device and method. The continuous annealing device comprises a heating section, a soaking section, a slow cooling section, a first rapid cooling section, a first aging section, a second rapid cooling section and a second aging section which are sequentially arranged. Wherein the heating section is used for heating strip steel; the soaking section is used for carrying out heat preservation treatment on the heated strip steel; the slow cooling section is used for carrying out primary cooling treatment on the strip steel subjected to heat preservation treatment at a first cooling speed; the first rapid cooling section is used for carrying out second cooling treatment on the strip steel subjected to the first cooling treatment at a second cooling speed; the first aging section is used for performing first aging treatment on the strip steel subjected to the second cooling treatment; the second rapid cooling section is used for carrying out third cooling treatment on the strip steel subjected to the first aging treatment at a third cooling speed; and the second aging section is used for carrying out second aging treatment on the strip steel subjected to third cooling treatment, and the second cooling speed and the third cooling speed are both higher than the first cooling speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of automobile steel and engineering structure steel, and in particular relates to a continuous annealing device and method. Background Art

[0002] With the development of the automobile industry and increasingly stringent government regulations, the automobile industry has an increasing demand for lightweight, high safety, low emissions and low costs. In order to reduce fuel consumption and improve safety, the strength grades of automobile parts are getting higher and higher, and the parts are becoming more and more complex. Typical grades of cold-rolled ultra-high strength steel include DP (Dual Phase) steel, TRIP (Transformation Induced Plasticity) steel, MS (Martensitic) steel, third-generation high-strength steel, etc. DP steel has been widely used in the automotive industry due to its good comprehensive mechanical properties, low alloy content and easy mass production. However, for some complex parts, DP steel has the defect of insufficient forming ability and is prone to cracking in areas with large strain. Common DP steel production processes include: Figure 1 As shown, it includes a heating section, a soaking section, a slow cooling section, a fast cooling section, an aging section and a final cooling section.

[0003] In order to cope with the problem of deformation of complex parts, advanced steel enterprises at home and abroad have successively developed the third generation of high-strength steel with excellent overall and local forming properties. The typical steel is QP (Quenching and Partitioning, quenching ductility) steel. Common QP steel production processes include Figure 2 As shown, it includes heating section, soaking section, slow cooling section, fast cooling section, aging section and final cooling section. The elongation of QP steel is significantly improved compared with DP steel. For example, the A80 of DP980 is generally around 13%, while the A80 of QP980 is as high as about 19%, which is more than 40% higher than DP980. However, as the requirements for forming performance of some car body parts become higher and higher, the traditional QP980 can no longer meet the relevant requirements. In addition, as the strength level of QP steel increases, its elongation gradually decreases, and it is difficult to meet the stamping requirements of complex parts. Based on this, how to further improve the forming performance of the third-generation high-strength steel is an urgent problem to be solved. Summary of the invention

[0004] The embodiments of the present application provide a continuous annealing device and method, aiming to further improve the formability of third-generation high-strength steel.

[0005] Other features and advantages of the present application will become apparent from the following detailed description, or may be learned in part by the practice of the present application.

[0006] According to a first aspect of the present application, a continuous annealing device is provided, comprising: a heating section, a soaking section, a slow cooling section, a first rapid cooling section, a first aging section, a second rapid cooling section and a second aging section arranged in sequence; wherein the heating section is used to heat the strip; the soaking section is used to keep the strip warm after the heating treatment; the slow cooling section is used to cool the strip at a first cooling rate for the first time after the keeping warm treatment; the first rapid cooling section is used to cool the strip at a second cooling rate for the second time after the first cooling treatment; the first aging section is used to age the strip at the first time after the second cooling treatment; the second rapid cooling section is used to cool the strip at a third cooling rate for the third time after the first aging treatment; and the second aging section is used to age the strip at the second time after the third cooling treatment, and the second cooling rate and the third cooling rate are both greater than the first cooling rate.

[0007] In some embodiments, the first quick cooling section includes a first quick cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling air duct, the second quick cooling section includes a second quick cooling fan, and the second aging section includes a second induction heater, a second radiation tube and a second cooling air duct; wherein the first radiation tube and the first cooling air duct are arranged between the first induction heater and the second quick cooling fan; and the second radiation tube and the second cooling air duct are arranged between the second induction heater and the rear aging equipment.

[0008] In some embodiments, the induction heating temperature range of the first induction heater is 0-800°C, the induction heating temperature range of the second induction heater is 0-500°C, and the cooling temperature ranges of the first fast cooling fan and the second fast cooling fan are both 0-800°C.

[0009] In some embodiments, the heating temperature range of the heating section is 0-950°C, the soaking time range of the soaking section is 0.5-5 min, the cooling temperature range of the slow cooling section is 0-200°C, and the aging time ranges of the first aging section and the second aging section are both 0.1-15 min.

[0010] In some embodiments, the continuous annealing device also includes: a first pyrometer, a second pyrometer, a third pyrometer, a fourth pyrometer, a fifth pyrometer, a sixth pyrometer, a seventh pyrometer, an eighth pyrometer and a ninth pyrometer; wherein the first pyrometer is arranged at the outlet of the heating section; the second pyrometer is arranged at the outlet of the soaking section; the third pyrometer is arranged at the outlet of the slow cooling section; the fourth pyrometer is arranged at the outlet of the first fast cooling section; the fifth pyrometer is arranged at the output end of the first induction heater; the sixth pyrometer is arranged at the outlet of the first aging section; the seventh pyrometer is arranged at the outlet of the second fast cooling section; the eighth pyrometer is arranged at the output end of the second induction heater; and the ninth pyrometer is arranged at the outlet of the second aging section.

[0011] In some embodiments, the continuous annealing device also includes: a rear-end aging device, which is connected to the outlet of the second aging section, and includes a final cooling section, a water quenching section, an outlet looper and a skin pass machine, or the rear-end aging device includes a third induction heater, a zinc pot, a post-plating cooling section, a water quenching section, an outlet looper and a skin pass machine.

[0012] According to the second aspect of the present application, a continuous annealing method is provided, which is applied to the above-mentioned continuous annealing device, and the continuous annealing method includes: controlling the heating section to heat the strip; controlling the soaking section to keep the strip after the heating treatment warm; controlling the slow cooling section to cool the strip after the keeping treatment for the first time at a first cooling rate; controlling the first rapid cooling section to cool the strip after the first cooling treatment for the second time at a second cooling rate; controlling the first aging section to age the strip after the second cooling treatment for the first time; controlling the second rapid cooling section to age the strip after the first aging treatment for the third time at a third cooling rate; and controlling the second aging section to age the strip after the third cooling treatment for the second time, wherein the second cooling rate and the third cooling rate are both greater than the first cooling rate.

[0013] In some embodiments, the first rapid cooling section includes a first rapid cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling duct, the second rapid cooling section includes a second rapid cooling fan, the second aging section includes a second induction heater, a second radiation tube and a second cooling duct, and after the slow cooling section is controlled to perform a first cooling treatment on the strip after the insulation treatment at a first cooling rate, the continuous annealing method further includes: turning on the first rapid cooling fan to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling rate; turning on or off the first induction heater, and controlling the first radiation tube or the first cooling duct to perform a first aging treatment on the strip after the second cooling treatment; turning on the second rapid cooling fan to perform a third cooling treatment on the strip after the first aging treatment at a third cooling rate; and turning on the second induction heater, and controlling the second radiation tube or the second cooling duct to perform a second aging treatment on the strip after the third cooling treatment.

[0014] In some embodiments, the first rapid cooling section includes a first rapid cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling duct, the second rapid cooling section includes a second rapid cooling fan, the second aging section includes a second induction heater, a second radiation tube and a second cooling duct, and after the slow cooling section is controlled to perform a first cooling treatment on the strip after the insulation treatment at a first cooling rate, the continuous annealing method further includes: turning on the first rapid cooling fan to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling rate; turning off the first induction heater, and controlling the first radiation tube or the first cooling duct to perform a first aging treatment on the strip after the second cooling treatment; and turning off the second rapid cooling fan and the second induction heater, and controlling the second radiation tube or the second cooling duct to perform a second aging treatment on the strip after the first aging treatment.

[0015] In some embodiments, the first rapid cooling section includes a first rapid cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling duct, the second rapid cooling section includes a second rapid cooling fan, the second aging section includes a second induction heater, a second radiation tube and a second cooling duct, and after the slow cooling section is controlled to perform a first cooling treatment on the strip after the insulation treatment at a first cooling rate, the continuous annealing method further includes: turning on the first rapid cooling fan to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling rate; turning on the first induction heater, and controlling the first radiation tube or the first cooling duct to perform a first aging treatment on the strip after the second cooling treatment; and turning off the second rapid cooling fan and the second induction heater, and controlling the second radiation tube or the second cooling duct to perform a second aging treatment on the strip after the first aging treatment.

[0016] The present application sequentially arranges a heating section, a soaking section, a slow cooling section, a first rapid cooling section, a first aging section, a second rapid cooling section and a second aging section in a continuous annealing device; wherein the heating section is used to heat the steel strip; the soaking section is used to heat the steel strip after the heating treatment; the slow cooling section is used to cool the steel strip after the heat treatment at a first cooling rate; the first rapid cooling section is used to cool the steel strip after the first cooling treatment at a second cooling rate; the first aging section is used to age the steel strip after the second cooling treatment; the second rapid cooling section is used to cool the steel strip after the first aging treatment at a third cooling rate; and the second aging section is used to age the steel strip after the third cooling treatment, and the second cooling rate and the third cooling rate are both greater than the first cooling rate. wherein, by adding the second rapid cooling section and the second aging section on the basis of the traditional continuous annealing production line, the elongation of the steel strip after annealing is significantly improved, the hole expansion rate is also improved, and the forming performance is significantly improved.

[0017] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present application, and together with the specification, are used to explain the principles of the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:

[0019] Figure 1A schematic diagram of a production process of DP steel in the related art is shown;

[0020] Figure 2 A schematic diagram of a production process of QP steel in the related art is shown;

[0021] Figure 3 A block diagram of a continuous annealing device according to some embodiments of the present disclosure is shown;

[0022] Figure 4 Shows Figure 3 A structural schematic diagram of a continuous annealing device;

[0023] Figure 5 Shown is applied to Figure 4 Schematic diagram of the production process of the continuous annealing device;

[0024] Figure 6 A schematic flow chart of a continuous annealing method according to some embodiments of the present disclosure is shown.

[0025] Description of Figure Numbers:

[0026] Label name Label name 1 Heating section 51 First induction heater 2 Soaking section 52 The first radiant tube 3 Slow cooling section 53 First cooling air duct 4 First fast cooling stage 61 Second fast cooling fan 5 The first validity period 71 Second induction heater 6 Second fast cooling stage 72 The second radiant tube 7 Second validity period 73 Second cooling air duct 31 Slow cooling fan I~IX The first pyrometer to the ninth pyrometer 41 First fast cooling fan DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0028] In addition, described feature, structure or characteristic can be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present application. However, those skilled in the art will appreciate that the technical scheme of the present application can be put into practice without one or more of the specific details, or other methods, components, devices, steps, etc. can be adopted. In other cases, known methods, devices, realizations or operations are not shown or described in detail to avoid blurring the various aspects of the application.

[0029] The flowcharts shown in the accompanying drawings are only exemplary and do not necessarily include all the contents and operations / steps, nor must they be executed in the order described. For example, some operations / steps can be decomposed, and some operations / steps can be combined or partially combined, so the actual execution order may change according to actual conditions.

[0030] It should also be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the objects used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those shown or described.

[0031] In order to further improve the formability of the third-generation automotive steel, a new annealing production line is needed. The domestic invention patent with application number CN105849289B proposes an annealing production line that can achieve the production of ultra-high-strength steel with excellent formability. This patent adds a heating table and a slow cooling or constant temperature holding table in front of the traditional annealing production line, which requires a very large transformation of the traditional annealing production line. Since the heating rate of the heating table is slow and the cooling rate of the slow cooling or constant temperature holding table is also slow, the annealing production line will be greatly lengthened and the cost of transformation is also very high. Since the annealing production line is long and the second cooling table in the annealing production line does not have induction heating capabilities, the annealing production line not only has a single type of annealing process that can be used, but also it is difficult to use the existing annealing process to produce high-strength steel (such as QP steel, etc.).

[0032] The present application provides a novel continuous annealing device, which adds a second rapid cooling section and a second aging section after the aging section of the traditional annealing production line, so that the elongation of the strip steel after annealing is significantly improved, and the hole expansion rate is also improved, so the forming performance is significantly improved. The continuous annealing device can produce DP steel, QP steel and other steel types according to the existing annealing process, and can also use a new annealing process to produce third-generation high-strength steel with higher elongation.

[0033] Figure 3 FIG. 4 is a block diagram of a continuous annealing device according to some embodiments of the present disclosure. Figure 3 As shown, in some embodiments, the continuous annealing device may include a heating section 1, a soaking section 2, a slow cooling section 3, a first rapid cooling section 4, a first aging section 5, a second rapid cooling section 6 and a second aging section 7 which are arranged in sequence; wherein the heating section 1 is used to heat the steel strip; the soaking section 2 is used to keep the steel strip warm after the heating treatment; the slow cooling section 3 is used to cool the steel strip after the keeping treatment for the first time at a first cooling rate; the first rapid cooling section 4 is used to cool the steel strip after the first cooling treatment for the second time at a second cooling rate; the first aging section 5 is used to cool the steel strip after the second cooling treatment for the first time; the second rapid cooling section 6 is used to cool the steel strip after the first aging treatment for the third time at a third cooling rate; and the second aging section 7 is used to cool the steel strip for the second time after the third cooling treatment, and both the second cooling rate and the third cooling rate are greater than the first cooling rate.

[0034] Figure 4 Shows Figure 3 A structural diagram of a continuous annealing device. Figure 3 and Figure 4 , the heating section 1 can use a heating device such as a radiant tube to heat the strip, and the heating temperature range can be 0-950°C. The soaking section 2 can also use a heating device such as a radiant tube to insulate the strip. The soaking section 2 should have good insulation capacity, and the soaking temperature fluctuation range should be less than or equal to ±5°C as much as possible. The soaking time range can be 0.5-5min. The slow cooling section 3 can use a slow cooling fan 31 to perform the first cooling treatment on the strip after the insulation treatment, so that the strip after the insulation treatment is slowly cooled. The cooling temperature range of the slow cooling section 3 can be controlled at 0-200°C.

[0035] In some embodiments, the first quick cooling section 4 may include a first quick cooling fan 41, the first aging section 5 may include a first induction heater 51, a first radiation tube 52 and a first cooling air duct 53, the second quick cooling section 6 may include a second quick cooling fan 61, and the second aging section 7 may include a second induction heater 71, a second radiation tube 72 and a second cooling air duct 73; wherein the first radiation tube 52 and the first cooling air duct 53 are arranged between the first induction heater 51 and the second quick cooling fan 61; and the second radiation tube 72 and the second cooling air duct 73 are arranged between the second induction heater 71 and the rear aging equipment (not shown).

[0036] It can be understood that the first rapid cooling section 4 can use the first rapid cooling fan 41 to perform a second cooling treatment on the strip after the first cooling treatment, so that the strip after the first cooling treatment can be quickly cooled, and the cooling temperature range of the first rapid cooling section can be 0-800°C.

[0037] The first aging section 5 can use the first induction heater 51, the first radiation tube 52 and the first cooling duct 53 to perform the first aging treatment on the strip steel after the second cooling treatment. The induction heating temperature range of the first induction heater 51 can be 0-800°C to meet the production process requirements of different steel grades. The aging time range of the first aging section 5 can be 0.1-15min. During the first aging treatment, the strip steel is heated by the first induction heater 51, and the temperature of the heated strip steel is kept constant by the first radiation tube 52 or the first cooling duct 53, so that the fluctuation range of the first aging temperature is as small as possible less than or equal to ±5°C.

[0038] The second rapid cooling section 6 can use the second rapid cooling fan 61 to perform a third cooling treatment on the strip after the first aging treatment, so as to quickly cool the strip after the first aging treatment. The cooling temperature range of the second rapid cooling section 6 can be the same as the induction heating temperature range of the first induction heater 51, that is, 0 to 800°C.

[0039] The second aging section 7 can use the second induction heater 71, the second radiation tube 72 and the second cooling duct 73 to perform a second aging treatment on the strip steel after the third cooling treatment. The induction heating temperature range of the second induction heater 71 can be 0-500°C, and the aging time range of the second aging section 7 can be 0.1-15min. During the second aging treatment, the strip steel is heated by the second induction heater 71, and the temperature of the heated strip steel is kept constant by the second radiation tube 72 or the second cooling duct 73, so that the fluctuation range of the second aging temperature is less than or equal to ±5°C as much as possible.

[0040] In some embodiments, the continuous annealing device may also include: a first pyrometer I, a second pyrometer II, a third pyrometer III, a fourth pyrometer IV, a fifth pyrometer V, a sixth pyrometer VI, a seventh pyrometer VII, an eighth pyrometer VIII and a ninth pyrometer IX; wherein the first pyrometer I is arranged at the outlet of the heating section 1; the second pyrometer II is arranged at the outlet of the soaking section 2; the third high temperature III is arranged at the outlet of the slow cooling section 3; the fourth high temperature IV is arranged at the outlet of the first rapid cooling section 4; the fifth pyrometer V is arranged at the output end of the first induction heater 51; the sixth pyrometer VI is arranged at the outlet of the first aging section 5; the seventh pyrometer VII is arranged at the outlet of the second rapid cooling section 6; the eighth pyrometer VIII is arranged at the output end of the second induction heater 71; and the ninth pyrometer IX is arranged at the outlet of the second aging section 7.

[0041] It should be noted that there are usually multiple first induction heaters in the first aging stage. In this case, the first induction heaters are usually arranged in series. If the first induction heater connected to the first fast cooling fan is used as the first first induction heater, the fifth pyrometer is arranged at the output end of the last first induction heater. Similarly, the eighth pyrometer is arranged at the output end of the last second induction heater.

[0042] It can be understood that the first pyrometer I is used to measure the heating temperature of the steel strip; the second pyrometer II is used to measure the even heat temperature of the steel strip; the third pyrometer III is used to measure the slow cooling temperature of the steel strip; the fourth pyrometer IV is used to measure the first rapid cooling temperature of the steel strip; the fifth pyrometer V is used to measure the first induction heating temperature of the steel strip; the sixth pyrometer VI is used to measure the first aging temperature of the steel strip; the seventh pyrometer VII is used to measure the second rapid cooling temperature of the steel strip; the eighth pyrometer VIII is used to measure the second induction heating temperature of the steel strip; and the ninth pyrometer IX is used to measure the second aging temperature of the steel strip.

[0043] In some embodiments, the continuous annealing device may further include: aging rear equipment, the aging rear equipment is connected to the outlet of the second aging section 7, the aging rear equipment includes a final cooling section, a water quenching section, an outlet looper and a skin pass machine, or the aging rear equipment includes an induction heater, a zinc pot, a post-plating cooling section, a water quenching section, an outlet looper and a skin pass machine.

[0044] It can be understood that the continuous annealing device can be used for both continuous annealing lines and galvanizing lines. When used in continuous annealing lines, the post-aging equipment may include a final cooling section, a water quenching section, an exit looper and a skin pass mill; when used in galvanizing lines, the post-aging equipment may include a third induction heater, a zinc pot, a post-plating cooling section, a water quenching section, an exit looper and a skin pass mill.

[0045] The continuous annealing device of the embodiment of the present application adds a second rapid cooling section and a second aging section after the aging section of the traditional annealing production line, so that the elongation of the strip steel after annealing is significantly improved, and the hole expansion rate is also improved, so the forming performance is significantly improved. The continuous annealing device can produce DP steel, QP steel and other steel types according to the existing annealing process, and can also use a new annealing process to produce third-generation high-strength steel with higher elongation.

[0046] Figure 6 FIG. 1 is a schematic diagram of a continuous annealing method according to some embodiments of the present disclosure. Figure 6 As shown, a continuous annealing method is provided, which is applied to the above-mentioned continuous annealing device. In some embodiments, the continuous annealing method may include the following steps:

[0047] Step 601, controlling the heating section to heat the steel strip;

[0048] Step 602, controlling the soaking section to perform heat preservation treatment on the heated strip;

[0049] Step 603, controlling the slow cooling section to perform a first cooling treatment on the steel strip after the insulation treatment at a first cooling rate;

[0050] Step 604, controlling the first rapid cooling section to perform a second cooling treatment at a second cooling rate on the strip after the first cooling treatment;

[0051] Step 605, controlling the first aging section to perform a first aging treatment on the steel strip after the second cooling treatment;

[0052] Step 606, controlling the second rapid cooling section to perform a third cooling treatment at a third cooling rate on the strip after the first aging treatment; and

[0053] Step 607, controlling the second aging section to perform a second aging treatment on the steel strip after the third cooling treatment, and the second cooling rate and the third cooling rate are both greater than the first cooling rate.

[0054] It is understandable that the production processes of different steel grades are different, and the control of the first aging stage, the second rapid cooling stage and the second aging stage is also different. The following introduces how to control the continuous annealing device to meet the production process requirements of different steel grades.

[0055] Figure 5 Shown is applied to Figure 4 Schematic diagram of the production process of the continuous annealing device. Figure 5 As shown in the figure, mode 1 is the production process of DP steel, mode 2 is the production process of QP steel, and modes 3 and 4 are the production processes of the third generation high-strength steel with higher formability. In these production processes, Ac1 is the starting temperature of pearlite to austenite transformation during heating, Ac3 is the final temperature of proeutectoid ferrite completely transformed into austenite during heating, and Ms is the starting temperature of martensite transformation during quenching.

[0056] For the production process of DP steel, in steps 604 to 607, the first rapid cooling fan can be turned on to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling rate; the first induction heater can be turned off, and the first radiation tube or the first cooling air duct can be controlled to perform a first aging treatment on the strip after the second cooling treatment; and the second rapid cooling fan and the second induction heater can be turned off, and the second radiation tube or the second cooling air duct can be controlled to perform a second aging treatment on the strip after the first aging treatment.

[0057] In this production process, the heating temperature, the soaking temperature and the slow cooling temperature are all consistent with the corresponding temperatures in the existing DP steel production process, the first rapid cooling temperature is the same as the rapid cooling temperature in the existing DP steel production process, the first aging temperature and the second aging temperature are the same as the aging temperatures in the existing DP steel production process, and the first induction heater of the first aging section, the second rapid cooling fan of the second rapid cooling section, and the second induction heater of the second aging section are not turned on.

[0058] For the production process of QP steel, in steps 604 to 607, the first rapid cooling fan can be turned on to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling rate; the first induction heater can be turned on, and the first radiation tube or the first cooling air duct can be controlled to perform a first aging treatment on the strip after the second cooling treatment; and the second rapid cooling fan and the second induction heater can be turned off, and the second radiation tube or the second cooling air duct can be controlled to perform a second aging treatment on the strip after the first aging treatment.

[0059] In this production process, the heating temperature, the soaking temperature and the slow cooling temperature are all consistent with the corresponding temperatures in the existing QP steel production process, the first rapid cooling temperature is the same as the rapid cooling temperature in the existing QP steel production process, the first aging temperature and the second aging temperature are the same as the aging temperatures in the existing QP steel production process, and the second rapid cooling fan of the second rapid cooling section and the second induction heater of the second aging section are not turned on.

[0060] For the production process of third-generation high-strength steel with higher formability, in steps 604 to 607, the first rapid cooling fan can be turned on to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling rate; the first induction heater can be turned on or off, and the first radiation tube or the first cooling air duct can be controlled to perform a first aging treatment on the strip after the second cooling treatment; the second rapid cooling fan can be turned on to perform a third cooling treatment on the strip after the first aging treatment at a third cooling rate; and the second induction heater can be turned on, and the second radiation tube or the second cooling air duct can be controlled to perform a second aging treatment on the strip after the third cooling treatment.

[0061] In the production process shown in Mode 3, the strip enters the first rapid cooling section after passing through the heating section, the soaking section and the slow cooling section, and the first rapid cooling fan, the first induction heater, the second rapid cooling fan and the second induction heater are all turned on.

[0062] In the production process shown in Mode 4, the strip enters the first rapid cooling section after passing through the heating section, the soaking section and the slow cooling section. The first rapid cooling fan, the second rapid cooling fan and the second induction heater are all turned on, and the first induction heater is turned off.

[0063] The continuous annealing method of the embodiment of the present application can be used to produce steel grades such as DP steel and QP steel, and can also be used to produce third-generation high-strength steel with higher elongation, and has good compatibility and practicality.

[0064] The following are application examples of the continuous annealing device involved in this application:

[0065] Conventional 780TR and 980TR slabs are cleaned and then hot-charged into a furnace for rolling. The slab heating temperature is set at 1150-1250°C, the final rolling temperature is set at 900°C, and the coiling temperature is set at 250°C to obtain hot-rolled plates.

[0066] The chemical composition of the slab can be found in Table 1 below, where 1# is 780TR and 2# is 980TR.

[0067] Table 1

[0068] Steel Type C,% Si, % Mn, % P,% S,% 1# 0.15 1.1 1.8 0.012 0.002 2# 0.18 1.3 2.0 0.011 0.003

[0069] The slab heating temperature is set to 1150-1250°C for structural homogenization and solid solution of micro-alloying elements. Too high a temperature may cause abnormal grain growth, while too low a temperature may cause uneven composition and insufficient solid solution of micro-alloying elements.

[0070] The final rolling temperature is set to 900℃ to ensure a good hot-rolled structure. If the final rolling temperature is too high, the grains may become coarse, and if the final rolling temperature is too low, mixed crystals may appear.

[0071] The coiling temperature is set at 600℃ for the convenience of rolling. Too high a coiling temperature will have an adverse effect on the control of the finished product surface.

[0072] The hot-rolled plate obtained by the above treatment is pickled to obtain a strip steel, and the strip steel is annealed using the above continuous annealing device. The annealing process parameters and mechanical properties are shown in Table 2.

[0073] Table 2

[0074]

[0075]

[0076] Examples 1 to 10 correspond to 1#780TR slabs. Example 1 corresponds to the production process of DP steel on a continuous annealing line. The yield strength and tensile strength of the strip steel after annealing under this process meet the performance requirements of DP780. Example 2 corresponds to the production process of TRIP steel on a continuous annealing line. The yield strength and tensile strength of the strip steel after annealing under this process meet the requirements of TRIP780. Example 3 corresponds to the production process of MS steel on a continuous annealing line. The performance of the strip steel after annealing under this process meets the requirements of MS1100. Example 4 also corresponds to the production process of MS steel on a continuous annealing line. The difference from Example 3 is that the second rapid cooling section and the second aging section are bypassed, shortening the aging time, and the tensile strength of the strip steel after annealing is slightly higher than that of Example 3. Example 5 corresponds to the production process of QP steel on a continuous annealing line. Compared with Example 2, the yield strength and tensile strength of the strip steel after annealing are not much different, but the elongation is increased to 22.3%, and the hole expansion rate is also significantly increased. Example 6 corresponds to the process of mode 3 on the continuous annealing line. In this embodiment, the first rapid cooling fan, the second rapid cooling fan, the first induction heater and the second induction heater are all turned on. Compared with Example 5, the yield strength and tensile strength of the strip after annealing are basically the same, but the elongation is significantly increased to 27%, and the hole expansion rate is also improved to a certain extent, which shows that the forming performance of the strip has been significantly improved. Example 7 shortens the aging time of the first aging stage and the second aging stage on the basis of Example 6, and the elongation of the strip after annealing is slightly reduced. Example 8 corresponds to the production process of QP steel on the galvanizing line. Example 9 is the application of the continuous annealing method of this application on the galvanizing line. Compared with Example 8, the elongation of the strip after annealing is significantly improved, and it is basically consistent with the change law of elongation in the application of the continuous annealing line. Example 10 corresponds to the process of mode 4 on the continuous annealing line. In this embodiment, the first rapid cooling fan, the second rapid cooling fan and the second induction heater are turned on. Compared with Example 5, the elongation of the strip after annealing is also significantly improved, and the hole expansion rate is also improved.

[0077] Examples 11 to 20 correspond to 2#980TR slabs. Example 11 corresponds to the production process of DP steel on a continuous annealing line. The yield strength and tensile strength of the strip steel after annealing under this process meet the performance requirements of DP980. Example 12 corresponds to the production process of TRIP steel on a continuous annealing line. The yield strength and tensile strength of the strip steel after annealing under this process both meet the requirements of TRIP980, and the elongation is improved compared with Example 11. Example 13 corresponds to the production process of MS steel on a continuous annealing line. The performance of the strip steel after annealing under this process meets the requirements of MS1180. Example 14 corresponds to the production process of MS steel on a continuous annealing line. The difference from Example 13 is that the second rapid cooling section and the second aging section are bypassed, shortening the aging time. Example 15 corresponds to the production process of QP steel on a continuous annealing line. Compared with Example 11, the elongation of the strip steel after annealing is increased to 18.5%, and the hole expansion rate is also significantly improved. Example 16 is the process of mode three on the continuous annealing line. Compared with Example 15, the yield strength and tensile strength of the strip after annealing are basically the same, but the elongation is significantly improved, and the hole expansion rate is also improved to a certain extent. Example 17 shortens the aging time of the first aging stage and the second aging stage on the basis of Example 16, and the elongation of the strip after annealing is slightly reduced. Example 18 corresponds to the production process of QP steel on the galvanizing line. Example 19 is the application of the continuous annealing method of the present application on the galvanizing line. Compared with Example 18, the elongation of the strip after annealing is significantly improved, and the hole expansion rate is also improved. Example 20 corresponds to the process of mode four on the continuous annealing line. Compared with Example 15, the elongation and hole expansion rate of the strip after annealing are improved.

[0078] It can be seen from the above embodiments that the continuous annealing device and method of the embodiments of the present application can be used for both continuous annealing lines and galvanizing lines; it can produce existing high-strength steels (such as DP steel, TRIP steel, MS steel, QP steel, etc.) according to existing processes, and can also produce third-generation high-strength steels with better forming performance according to new annealing processes (such as mode three and mode four).

[0079] The above description is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of the claims of the present application.

Claims

1. A continuous annealing device, characterized in that: include: The heating section, soaking section, slow cooling section, first rapid cooling section, first aging section, second rapid cooling section and second aging section are arranged in sequence; wherein, The heating section is used to heat the steel strip; The soaking section is used to perform heat preservation treatment on the strip steel after the heating treatment; The slow cooling section is used to perform a first cooling treatment on the steel strip after the heat preservation treatment at a first cooling speed; The first rapid cooling section is used to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling rate; The first aging section is used to perform a first aging treatment on the steel strip after the second cooling treatment; The second rapid cooling section is used to perform a third cooling treatment at a third cooling rate on the strip after the first aging treatment; as well as The second aging section is used to perform a second aging treatment on the steel strip after the third cooling treatment, and the second cooling rate and the third cooling rate are both greater than the first cooling rate.

2. The continuous annealing device according to claim 1, characterized in that: The first fast cooling section includes a first fast cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling air duct, the second fast cooling section includes a second fast cooling fan, and the second aging section includes a second induction heater, a second radiation tube and a second cooling air duct; wherein, The first radiation tube and the first cooling air duct are arranged between the first induction heater and the second fast cooling fan; and The second radiation tube and the second cooling air duct are arranged between the second induction heater and the aging rear equipment.

3. The continuous annealing device according to claim 2, characterized in that: The induction heating temperature range of the first induction heater is 0-800°C, the induction heating temperature range of the second induction heater is 0-500°C, and the cooling temperature ranges of the first fast cooling fan and the second fast cooling fan are both 0-800°C.

4. The continuous annealing device according to claim 2, characterized in that: The heating temperature range of the heating section is 0-950°C, the soaking time range of the soaking section is 0.5-5min, the cooling temperature range of the slow cooling section is 0-200°C, and the aging time ranges of the first aging section and the second aging section are both 0.1-15min.

5. The continuous annealing device according to claim 2, characterized in that: Also includes: a first pyrometer, a second pyrometer, a third pyrometer, a fourth pyrometer, a fifth pyrometer, a sixth pyrometer, a seventh pyrometer, an eighth pyrometer, and a ninth pyrometer; wherein, The first pyrometer is disposed at the outlet of the heating section; The second pyrometer is disposed at the outlet of the soaking section; The third pyrometer is arranged at the outlet of the slow cooling section; The fourth pyrometer is arranged at the outlet of the first rapid cooling section; The fifth pyrometer is disposed at the output end of the first induction heater; The sixth pyrometer is disposed at the outlet of the first aging section; The seventh pyrometer is arranged at the outlet of the second fast cooling section; The eighth pyrometer is disposed at the output end of the second induction heater; and The ninth pyrometer is disposed at the outlet of the second aging section.

6. The continuous annealing device according to claim 1, characterized in that: Also includes: The rear-end equipment of aging is connected to the outlet of the second aging section, and includes a final cooling section, a water quenching section, an outlet looper and a skin pass mill, or the rear-end equipment of aging includes a third induction heater, a zinc pot, a post-plating cooling section, a water quenching section, an outlet looper and a skin pass mill.

7. A continuous annealing method, characterized in that: Applied to the continuous annealing device according to any one of claims 1 to 6, the continuous annealing method comprises: Control the heating section to heat the strip; Control the soaking section to keep the strip warm after heating; Controlling the slow cooling section to perform a first cooling treatment on the steel strip after the insulation treatment at a first cooling speed; Controlling the first rapid cooling section to perform a second cooling treatment on the strip after the first cooling treatment at a second cooling speed; Controlling the first aging stage to perform the first aging treatment on the strip after the second cooling treatment; Controlling the second rapid cooling section to perform a third cooling treatment on the strip after the first aging treatment at a third cooling rate; and The second aging section is controlled to perform a second aging treatment on the steel strip after the third cooling treatment, and the second cooling rate and the third cooling rate are both greater than the first cooling rate.

8. The continuous annealing method according to claim 7, characterized in that: The first rapid cooling section includes a first rapid cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling duct, the second rapid cooling section includes a second rapid cooling fan, the second aging section includes a second induction heater, a second radiation tube and a second cooling duct, and after the controlled slow cooling section performs a first cooling treatment on the heat-insulated strip at a first cooling speed, the continuous annealing method further includes: Turning on the first rapid cooling fan to perform a second cooling treatment on the steel strip after the first cooling treatment at a second cooling speed; Turning on or off the first induction heater, and controlling the first radiation tube or the first cooling air duct to perform a first aging treatment on the steel strip after the second cooling treatment; Turning on the second rapid cooling fan to perform a third cooling treatment at a third cooling rate on the steel strip after the first aging treatment; and The second induction heater is turned on, and the second radiation tube or the second cooling air duct is controlled to perform a second aging treatment on the steel strip after the third cooling treatment.

9. The continuous annealing method according to claim 8, characterized in that: The first rapid cooling section includes a first rapid cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling duct, the second rapid cooling section includes a second rapid cooling fan, the second aging section includes a second induction heater, a second radiation tube and a second cooling duct, and after the controlled slow cooling section performs a first cooling treatment on the heat-insulated strip at a first cooling speed, the continuous annealing method further includes: Turning on the first rapid cooling fan to perform a second cooling treatment on the steel strip after the first cooling treatment at a second cooling speed; turning off the first induction heater and controlling the first radiation tube or the first cooling air duct to perform a first aging treatment on the steel strip after the second cooling treatment; and The second rapid cooling fan and the second induction heater are turned off, and the second radiation tube or the second cooling air duct is controlled to perform a second aging treatment on the steel strip after the first aging treatment.

10. The continuous annealing method according to claim 7, characterized in that: The first rapid cooling section includes a first rapid cooling fan, the first aging section includes a first induction heater, a first radiation tube and a first cooling duct, the second rapid cooling section includes a second rapid cooling fan, the second aging section includes a second induction heater, a second radiation tube and a second cooling duct, and after the controlled slow cooling section performs a first cooling treatment on the heat-insulated strip at a first cooling speed, the continuous annealing method further includes: Turning on the first rapid cooling fan to perform a second cooling treatment on the steel strip after the first cooling treatment at a second cooling speed; Turning on the first induction heater and controlling the first radiation tube or the first cooling air duct to perform a first aging treatment on the steel strip after the second cooling treatment; and The second rapid cooling fan and the second induction heater are turned off, and the second radiation tube or the second cooling air duct is controlled to perform a second aging treatment on the steel strip after the first aging treatment.

Citation Information

Patent Citations

  • Continuous annealing furnace of high-efficiency energy-saving metal strip

    CN102010981A

  • High-plasticity 700 MPa cold-rolled weather-proof dual-phase steel and preparation method thereof

    CN105063510A

  • Production method of SEDDQ steel

    CN108796204A

  • Cu-Ti-P-Ni-Er copper alloy material and preparation method thereof

    CN112359246A

  • Preparation method and application of DP980 chilled steel strip

    CN113957221A

Cited By

  • Continuous annealing device and method

    WO2026051249A1