Production process of aluminum beryllium intermediate alloy
By combining slow natural cooling and fast cooling processes, combined with hydrothermal treatment and porous microsphere synthesis refining agent, the performance problems caused by the difference in melting point in the preparation of aluminum beryllium intermediate alloy are solved, and the stress relaxation resistance of aluminum beryllium intermediate alloy is improved and Mechanical properties and achieve environmentally friendly and efficient refining effect.
Patent Information
- Application Number
- CN202411571212.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-03
AI Technical Summary
In the preparation process of existing aluminum-beryllium intermediate alloys, due to the large difference in melting points between beryllium and aluminum, it leads to eutectic reactions, high alumina content, and metal oxide slag inclusions, which affects the density, ductility and hardness of the alloy, and is melted. Improper time will lead to segregation, pore defects and dendrites, affecting performance.
Using a combination of slow natural cooling and rapid cooling technology, porous carbon microspheres are obtained by grasping the rapid cooling timing, combining the use of refining agents, including hydrothermal treatment-synthesis of tanninic acid/iron microspheres and potassium hydroxide carbonization, and the porous carbon microspheres are obtained. Magnesium oxalate is synthesized on the surface of porous microspheres to produce carbon monoxide gas to remove active hydrogen, increase the adsorption and binding rate of oxygen impurities, and produce an aluminum beryllium intermediate alloy.
Reduce segregation of beryllium, improve the stress relaxation resistance of aluminum beryllium intermediate alloy, enhance the mechanical properties, and the refining process is environmentally friendly and chlorine-free release.
Smart Images

Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy smelting, and in particular to a production process of an aluminum-beryllium master alloy. Background Art
[0002] In the aluminum alloy smelting process, most alloying elements are added in the form of master alloys. However, the melting points of some metal elements are very different from those of the alloy, so a large amount of metal elements need to be lost when added to the alloy, or sometimes even cannot be added. For example, the melting point of beryllium is much higher than the melting point of cast aluminum alloy. If beryllium is directly added to the alloy, it cannot be melted. Generally, beryllium and other elements are made into a composite melt with a melting point close to that of the working alloy, and then smelted later.
[0003] In the current prior art, the preparation process of aluminum-beryllium master alloy mainly involves placing the melt of beryllium and aluminum in a furnace and melting and mixing them under the action of a protective agent or a protective atmosphere. However, the melting points of beryllium and aluminum are quite different, with the melting point of beryllium at 1280°C and the melting point of aluminum at 660°C. And from the phase diagram of beryllium-aluminum, it can be seen that the alloy actually undergoes a eutectic reaction at around 650°C, and is not a pure phase material. In addition, the length of the smelting time and solidification time has an impact on the performance of the aluminum-beryllium master alloy: when the smelting temperature is higher than the melting point of aluminum, the longer the smelting time, the higher the alumina content. The formation of metal oxide inclusions will affect the performance of the aluminum-beryllium master alloy, reducing the density, ductility and hardness of the alloy; if the smelting time is too short, the beryllium particles in the aluminum-beryllium master alloy will be uneven in size and may be accompanied by micropore defects, which will affect the performance of the alloy; if the solidification time is too short, coarse particles or lamellar structures with various anisotropies will appear, and micropore defects will also occur; if the solidification time is too long, the two phases of beryllium and aluminum will separate, resulting in dendrites and segregation, causing performance deterioration or even unusability. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a production process of aluminum-beryllium master alloy.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A production process of aluminum-beryllium master alloy comprises the following steps:
[0007] S1. Weigh the following raw materials in parts by weight: 0.1-0.15 parts of tin, 0.2-0.4 parts of zinc, 1-3 parts of beryllium, 95-98 parts of aluminum, and 0.3-0.5 parts of refining agent;
[0008] S2, heating beryllium until it is melted, adding tin and zinc while stirring, and continuing to stir until they are melted after they are completely added to obtain a composite melt for later use;
[0009] S3, heating aluminum to melt to obtain aluminum melt. Then raising the temperature to 1200°C, slowly adding the composite melt while stirring, adding the refining agent after slagging, transferring to a casting mold after refining for 3-5 hours, cooling naturally to 800-900°C and then rapidly cooling to room temperature to obtain aluminum-beryllium master alloy.
[0010] By combining slow natural cooling with rapid cooling processes and effectively controlling the timing of starting rapid cooling, beryllium segregation can be reduced, making the aluminum-beryllium master alloy exhibit excellent stress relaxation resistance.
[0011] Furthermore, the refining agent is prepared by the following steps:
[0012] Step 1: Add tannic acid to deionized water, stir at a uniform speed to obtain a tannic acid aqueous solution for later use. Control the dosage ratio of tannic acid to deionized water to be 1-2g:20mL; Add ferric nitrate nonahydrate to deionized water, stir evenly to obtain a ferric nitrate aqueous solution for later use. Control the dosage ratio of ferric nitrate nonahydrate to deionized water to be 1.5-2g:20mL; Add the ferric nitrate aqueous solution dropwise to the tannic acid aqueous solution, heat to 120-140°C, hydrothermally treat for 12h, wash and dry to obtain microspheres;
[0013] Step 2: Mix the prepared microspheres and potassium hydroxide evenly, introduce nitrogen, heat to 720-750℃, and carbonize for 2h. Then wash three times with 10% dilute hydrochloric acid solution and deionized water respectively to obtain porous microspheres. The weight ratio of microspheres to potassium hydroxide is controlled to be 1:1;
[0014] Step 3: Add sodium oxalate and magnesium chloride hexahydrate into deionized water, stir at a uniform speed and add porous microspheres, heat to 100-110°C, keep warm for 2.5 hours, take out the sample after the reaction, wash it three times with deionized water, and vacuum dry it at 65°C for 12 hours to obtain a refining agent. The weight ratio of sodium oxalate, magnesium chloride hexahydrate, porous microspheres and deionized water is controlled to be 1:1:5:10.
[0015] In the first step, hydrothermal treatment is used to synthesize tannic acid / iron microspheres. There is a strong complexation between iron ions and tannic acid, so that iron atoms can be evenly dispersed in the microspheres; in the second step, potassium hydroxide is used to carbonize to obtain porous carbon microspheres. Due to the etching effect of potassium hydroxide, the surface of the microspheres becomes rougher and the specific surface area is increased; in the third step, sodium oxalate and magnesium chloride hexahydrate are used as raw materials, and magnesium oxalate is synthesized in the pores on the surface of the porous microspheres by a hydrothermal method to obtain a refining agent. When the refining agent is used, magnesium oxalate decomposes at high temperature to generate carbon monoxide gas, which can undergo redox reaction with active hydrogen, thereby quickly removing active hydrogen in high-temperature aluminum liquid, and no chlorine is released during the reaction, which is more environmentally friendly. The remaining porous microspheres have a large specific surface area, which can increase their adsorption and binding speed with oxygen impurities, playing a role in efficient refining.
[0016] Beneficial effects of the present invention:
[0017] The present invention prepares an aluminum-beryllium master alloy. The production process adopts a combination of slow natural cooling and rapid cooling processes. By effectively grasping the start time of rapid cooling, the segregation of beryllium can be reduced, so that the aluminum-beryllium master alloy exhibits excellent stress relaxation resistance.
[0018] The present invention also prepares a refining agent, which first uses hydrothermal treatment to synthesize tannic acid / iron microspheres. There is a strong complexation between iron ions and tannic acid, so that iron atoms can be evenly dispersed in the microspheres; then potassium hydroxide is used for one-step carbonization to obtain porous carbon microspheres. Due to the etching effect of potassium hydroxide, the surface of the microspheres becomes rougher, and the specific surface area is increased; finally, sodium oxalate and magnesium chloride hexahydrate are used as raw materials, and magnesium oxalate is synthesized in the pores on the surface of the porous microspheres by a hydrothermal method, thereby preparing a refining agent. When the refining agent is used, the magnesium oxalate therein decomposes at high temperature to generate carbon monoxide gas, which can undergo an oxidation-reduction reaction with active hydrogen, thereby quickly removing active hydrogen in high-temperature aluminum liquid, and no chlorine is released during the reaction process, which is more environmentally friendly. The remaining porous microspheres have an ultra-large specific surface area, which can increase their adsorption and binding speed with oxygen impurities, and play a role in efficient refining. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] A production process of aluminum-beryllium master alloy comprises the following steps:
[0022] S1. Weigh the following raw materials in parts by weight: 0.1 parts of tin, 0.2 parts of zinc, 1 part of beryllium, 95 parts of aluminum, and 0.3 parts of refining agent;
[0023] S2, heating beryllium until it is melted, adding tin and zinc while stirring, and continuing to stir until they are melted after they are completely added to obtain a composite melt for later use;
[0024] S3, heating aluminum to melt to obtain aluminum melt. Then raising the temperature to 1200°C, slowly adding the composite melt while stirring, adding the refining agent after slagging, transferring to a casting mold after refining for 3 hours, cooling naturally to 800°C and then rapidly cooling to room temperature to obtain aluminum-beryllium master alloy.
[0025] The refining agent is prepared by the following steps:
[0026] Step 1: Add tannic acid to deionized water and stir at a uniform speed to obtain a tannic acid aqueous solution for later use. Control the dosage ratio of tannic acid to deionized water to be 1g:20mL; Add ferric nitrate nonahydrate to deionized water and stir evenly to obtain a ferric nitrate aqueous solution for later use. Control the dosage ratio of ferric nitrate nonahydrate to deionized water to be 1.5g:20mL; Add the ferric nitrate aqueous solution dropwise to the tannic acid aqueous solution, heat to 120°C, hydrothermally treat for 12h, wash and dry to obtain microspheres;
[0027] Step 2: Mix the prepared microspheres and potassium hydroxide evenly, introduce nitrogen, heat to 720°C, and carbonize for 2 hours. Then, wash three times with 10% dilute hydrochloric acid solution and deionized water respectively to obtain porous microspheres. The weight ratio of microspheres to potassium hydroxide is controlled to be 1:1;
[0028] Step 3: Add sodium oxalate and magnesium chloride hexahydrate into deionized water, stir at a uniform speed and add porous microspheres, heat to 100°C, keep warm for 2.5 hours, take out the sample after the reaction, wash it three times with deionized water, and vacuum dry it at 65°C for 12 hours to obtain a refining agent. The weight ratio of sodium oxalate, magnesium chloride hexahydrate, porous microspheres and deionized water is controlled to be 1:1:5:10.
[0029] Example 2
[0030] A production process of aluminum-beryllium master alloy comprises the following steps:
[0031] S1. Weigh the following raw materials in parts by weight: 0.12 parts of tin, 0.2 parts of zinc, 2 parts of beryllium, 96 parts of aluminum, and 0.4 parts of refining agent;
[0032] S2, heating beryllium until it is melted, adding tin and zinc while stirring, and continuing to stir until they are melted after they are completely added to obtain a composite melt for later use;
[0033] S3, heating aluminum to melt to obtain aluminum melt. Then raising the temperature to 1200°C, slowly adding the composite melt while stirring, adding the refining agent after slagging, transferring to a casting mold after refining for 3 hours, cooling naturally to 850°C and then rapidly cooling to room temperature to obtain aluminum-beryllium master alloy.
[0034] The refining agent is prepared by the following steps:
[0035] Step 1: Add tannic acid to deionized water and stir at a uniform speed to obtain a tannic acid aqueous solution for later use. Control the dosage ratio of tannic acid to deionized water to be 1.5 g:20 mL; Add ferric nitrate nonahydrate to deionized water and stir evenly to obtain a ferric nitrate aqueous solution for later use. Control the dosage ratio of ferric nitrate nonahydrate to deionized water to be 1.8 g:20 mL; Add the ferric nitrate aqueous solution dropwise to the tannic acid aqueous solution, heat to 130°C, hydrothermally treat for 12 hours, wash and dry to obtain microspheres;
[0036] Step 2: Mix the prepared microspheres and potassium hydroxide evenly, introduce nitrogen, heat to 730°C, and carbonize for 2 hours. Then, wash three times with 10% dilute hydrochloric acid solution and deionized water respectively to obtain porous microspheres. The weight ratio of microspheres to potassium hydroxide is controlled to be 1:1;
[0037] Step 3: Add sodium oxalate and magnesium chloride hexahydrate into deionized water, stir at a uniform speed and add porous microspheres, heat to 105°C, keep warm for 2.5 hours, take out the sample after the reaction, wash it three times with deionized water, and vacuum dry it at 65°C for 12 hours to obtain a refining agent. The weight ratio of sodium oxalate, magnesium chloride hexahydrate, porous microspheres and deionized water is controlled to be 1:1:5:10.
[0038] Example 3
[0039] A production process of aluminum-beryllium master alloy comprises the following steps:
[0040] S1. Weigh the following raw materials in parts by weight: 0.14 parts of tin, 0.4 parts of zinc, 2 parts of beryllium, 98 parts of aluminum, and 0.5 parts of refining agent;
[0041] S2, heating beryllium until it is melted, adding tin and zinc while stirring, and continuing to stir until they are melted after they are completely added to obtain a composite melt for later use;
[0042] S3, heating aluminum to melt to obtain aluminum melt. Then raising the temperature to 1200°C, slowly adding the composite melt while stirring, adding the refining agent after slagging, transferring to a casting mold after refining for 5 hours, cooling naturally to 900°C and then rapidly cooling to room temperature to obtain aluminum-beryllium master alloy.
[0043] The refining agent is prepared by the following steps:
[0044] Step 1: Add tannic acid to deionized water, stir at a constant speed to obtain a tannic acid aqueous solution for later use. Control the dosage ratio of tannic acid to deionized water to be 1.8 g: 20 mL; Add ferric nitrate nonahydrate to deionized water, stir evenly to obtain a ferric nitrate aqueous solution for later use. Control the dosage ratio of ferric nitrate nonahydrate to deionized water to be 1.8 g: 20 mL; Add the ferric nitrate aqueous solution dropwise to the tannic acid aqueous solution, heat to 140°C, hydrothermally treat for 12 hours, wash and dry to obtain microspheres;
[0045] Step 2: Mix the prepared microspheres and potassium hydroxide evenly, introduce nitrogen, heat to 740°C, and carbonize for 2 hours. Then, wash with 10% dilute hydrochloric acid solution and deionized water three times to obtain porous microspheres. The weight ratio of microspheres to potassium hydroxide is controlled to be 1:1;
[0046] Step 3: Add sodium oxalate and magnesium chloride hexahydrate into deionized water, stir at a uniform speed and add porous microspheres, heat to 110°C, keep warm for 2.5 hours, take out the sample after the reaction, wash it three times with deionized water, and vacuum dry it at 65°C for 12 hours to obtain a refining agent. The weight ratio of sodium oxalate, magnesium chloride hexahydrate, porous microspheres and deionized water is controlled to be 1:1:5:10.
[0047] Example 4
[0048] A production process of aluminum-beryllium master alloy comprises the following steps:
[0049] S1. Weigh the following raw materials in parts by weight: 0.15 parts of tin, 0.4 parts of zinc, 3 parts of beryllium, 98 parts of aluminum, and 0.5 parts of refining agent;
[0050] S2, heating beryllium until it is melted, adding tin and zinc while stirring, and continuing to stir until they are melted after they are completely added to obtain a composite melt for later use;
[0051] S3, heating aluminum to melt to obtain aluminum melt. Then raising the temperature to 1200°C, slowly adding the composite melt while stirring, adding the refining agent after slagging, transferring to a casting mold after refining for 5 hours, cooling naturally to 900°C and then rapidly cooling to room temperature to obtain aluminum-beryllium master alloy.
[0052] The refining agent is prepared by the following steps:
[0053] Step 1: Add tannic acid to deionized water, stir at a constant speed to obtain a tannic acid aqueous solution for later use. Control the dosage ratio of tannic acid to deionized water to be 2g:20mL; Add ferric nitrate nonahydrate to deionized water, stir evenly to obtain a ferric nitrate aqueous solution for later use. Control the dosage ratio of ferric nitrate nonahydrate to deionized water to be 2g:20mL; Add the ferric nitrate aqueous solution dropwise to the tannic acid aqueous solution, heat to 140°C, hydrothermally treat for 12h, wash and dry to obtain microspheres;
[0054] Step 2: Mix the prepared microspheres and potassium hydroxide evenly, introduce nitrogen, heat to 750°C, and carbonize for 2 hours. Then, wash three times with 10% dilute hydrochloric acid solution and deionized water respectively to obtain porous microspheres. The weight ratio of microspheres to potassium hydroxide is controlled to be 1:1;
[0055] Step 3: Add sodium oxalate and magnesium chloride hexahydrate into deionized water, stir at a uniform speed and add porous microspheres, heat to 110°C, keep warm for 2.5 hours, take out the sample after the reaction, wash it three times with deionized water, and vacuum dry it at 65°C for 12 hours to obtain a refining agent. The weight ratio of sodium oxalate, magnesium chloride hexahydrate, porous microspheres and deionized water is controlled to be 1:1:5:10.
[0056] Comparative Example 1
[0057] Compared with Example 1, this comparative example does not add a refining agent, and the rest is the same as Example 1.
[0058] Comparative Example 2
[0059] Compared with Example 1, this comparative example uses magnesium oxalate as a refining agent, and the rest is the same as Example 1.
[0060] The properties of the aluminum-beryllium master alloys prepared in Examples 1-4 and Comparative Examples 1-2 were tested, and the results are shown in Table 1 below, where:
[0061] Tensile Strength: Tested according to standard GB / T 228.1-2010.
[0062] Yield Strength: Tested according to standard GB / T 228.1-2010.
[0063] Stress relaxation resistance: tested according to GB / T 2039, with a loading stress of 800MPa. After the alloy was stress relaxed at 250℃ for 100h, the initial stress and the residual stress after 100h were calculated according to the following formula:
[0064] ,in represents the initial stress, It represents the residual stress after time t (100h).
[0065] The smaller the relaxation rate, the better the alloy's stress relaxation resistance.
[0066] Table 1
[0067]
[0068] It can be seen from Table 1 above that the aluminum-beryllium master alloys prepared in Examples 1-4 of the present invention have better mechanical properties and better stress relaxation resistance.
[0069] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A production process of aluminum-beryllium master alloy, characterized in that: The steps include: S1. Weigh the following raw materials in parts by weight: 0.1-0.15 parts of tin, 0.2-0.4 parts of zinc, 1-3 parts of beryllium, 95-98 parts of aluminum, and 0.3-0.5 parts of refining agent; S2, heating beryllium until it is melted, adding tin and zinc while stirring, and continuing to stir until they are melted after they are completely added to obtain a composite melt for later use; S3, heating aluminum to melt to obtain aluminum melt, then heating to 1200°C, slowly adding composite melt while stirring, adding refining agent after slagging, transferring to a casting mold after refining for 3-5h, naturally cooling to 800-900°C and then rapidly cooling to room temperature to obtain aluminum-beryllium master alloy; The refining agent is prepared by the following steps: Step 1: Add tannic acid to deionized water, stir at a uniform speed to obtain a tannic acid aqueous solution for later use; add ferric nitrate nonahydrate to deionized water, stir evenly to obtain a ferric nitrate aqueous solution for later use; add the ferric nitrate aqueous solution dropwise to the tannic acid aqueous solution, heat to 120-140° C., perform hydrothermal treatment for 12 hours, wash and dry to obtain microspheres; Step 2: The prepared microspheres and potassium hydroxide are mixed evenly, nitrogen is introduced, the temperature is raised to 720-750°C, and carbonization is carried out for 2 hours. After that, porous microspheres are obtained by washing with 10% by mass dilute hydrochloric acid solution and deionized water three times respectively; Step 3: Add sodium oxalate and magnesium chloride hexahydrate into deionized water, stir at a uniform speed and add porous microspheres, raise the temperature to 100-110°C, and keep the temperature to react for 2.5 hours. After the reaction is completed, take out the sample, wash it three times with deionized water, and vacuum dry it at 65°C for 12 hours to obtain a refining agent.
2. The production process of an aluminum-beryllium master alloy according to claim 1, characterized in that: In the first step, the dosage ratio of tannic acid to deionized water is controlled to be 1-2 g: 20 mL, and the dosage ratio of ferric nitrate nonahydrate to deionized water is controlled to be 1.5-2 g: 20 mL.
3. The production process of an aluminum-beryllium master alloy according to claim 1, characterized in that: In the second step, the weight ratio of the microspheres to potassium hydroxide is controlled to be 1:
1.
4. The production process of an aluminum-beryllium master alloy according to claim 1, characterized in that: In the third step, the weight ratio of sodium oxalate, magnesium chloride hexahydrate, porous microspheres and deionized water is controlled to be 1:1:5:10.
Citation Information
Patent Citations
Smelting preparation method of heat insulation aluminum alloy profile
CN103103416A
Aluminum alloy material capable of improving impact resistance for cylinder cover and manufacturing method of aluminum alloy material
CN104862544A
Diamond enhanced multicomponent aluminum silicon copper alloy material for cylinder cover and preparation method of material
CN104862545A
Aluminum alloy material reasonable in proportion and preparation method thereof
CN105525118A
Aluminum beryllium intermediate alloy and preparation method thereof
CN115287503A
Cited By
Production process of beryllium aluminum alloy with high beryllium content
CN119351817A
Production process of high-beryllium-content beryllium-aluminum alloy
CN119351817B